◆ Rebuild

Part 13 · Electricity

The Battery

How to make electricity from two different metals and a salty or sour liquid — Volta's pile, the cup battery, and the steady Daniell cell — and how to test it with no meter. The first source of steady electric current.

Difficulty
●●●●●
Time
An afternoon for a pile once you have zinc and copper; a week for a bank of Daniell cells
Steps from zero
13 prerequisites →

You need first

Copper SmeltingFermentation

This unlocks

Electric Bells, Buzzers and AlarmsDry Cells and Electric TorchesElectrolysisThe ElectromagnetThe Induction CoilThe Rechargeable BatteryThe Light BulbElectroplating

Raw materials

salt
The full path from nothing — 13 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Fermentation
  12. Bellows
  13. Copper Smelting
  14. The Battery

Do them roughly in this order. See it on the tech tree →

Why it matters

A battery gives you a steady flow of electricity that you can switch on and off and lead along a wire. With it you can make an The Electromagnet, send messages by The Telegraph, split water and salt into new substances by Electrolysis, coat metals with copper or silver (Electroplating), refine pure copper for Copper Wire, and make your first electric light.

Before 1800 people knew electricity only as sparks from rubbed amber and glass — a brief jolt, then nothing. Volta's battery changed that in a single year. Within months people were using it to discover new chemical elements. It remained the only practical source of electric current until the The Generator arrived some 70 years later, and it is still the right tool wherever you need a little electricity, steadily, with no moving parts.

How it works

Electricity is a flow of tiny charged particles called electrons. In a metal wire, they can drift along freely. To make them flow, you need something that pushes them in at one end of the wire and takes them out at the other.

A cell — one unit of a battery — does this with three things:

  1. A metal that dissolves easily, such as zinc. When zinc dissolves in a salty or sour liquid, each zinc atom leaves behind electrons in the metal. The zinc plate becomes crowded with electrons: it is the negative end (−).
  2. A metal that does not dissolve easily, such as copper. It is the positive end (+).
  3. An electrolyte — a liquid that carries electric charge but is not a metal: salt water (brine), vinegar or dilute acid. It completes the loop inside the cell.

Join the two plates with a wire outside the liquid and electrons flow from the zinc, through the wire, to the copper. The zinc slowly dissolves to pay for it. No zinc used up, no electricity. A battery is really a slow, controlled fire of zinc, giving out electricity instead of heat.

Two words you need:

  • Voltage (measured in volts, V) is the push. Think of it as the height a waterfall drops. It depends only on which two metals you use, not on their size.
  • Current (measured in amperes or amps, A) is how much electricity flows — the amount of water going over the falls. Bigger plates, closer together, in a stronger electrolyte, give more current.

Which metals

The further apart two metals are in this list, the more voltage they give together. The one higher in the list dissolves and becomes the negative plate.

Pair (negative / positive) Volts per cell, roughly Comment
Zinc / copper 0.8–1.0 The standard. Use this if at all possible
Zinc / dense carbon 1.0–1.3 Hard coke or graphite instead of copper works well
Iron / copper 0.3–0.5 Works, but you need two to three times as many cells
Zinc / iron about 0.4 Weak
Tin / copper 0.1 or less Hardly worth it
Copper / copper 0 Two plates of the same metal give nothing

These are "open-circuit" figures — the push with nothing connected. As soon as current flows, the voltage sags (see polarisation below).

Series and parallel

One cell gives less than a volt. To get more push, connect cells in series: the copper of one to the zinc of the next, in a chain. Their voltages add. Ten zinc–copper cells in series give about 9 V.

To get more current at the same voltage, connect cells in parallel: all the zincs joined together, all the coppers joined together. Or simply use bigger plates.

− + +− IN SERIES copper to the next zinc: volts add up 4 cells × 0.9 V ≈ 3.6 V IN PARALLEL zincs together, coppers together: still 0.9 V, but 4 times the current, or 4 times as long zinc (grey) · copper (orange) · electrolyte (blue)
Fig. 1 Series and parallel. In series (left), each cell's copper is joined to the next cell's zinc and the voltages add up. In parallel (right), all the zincs are joined and all the coppers are joined; the voltage stays the same but the battery can supply more current for longer.

Polarisation: why simple cells fade

In a simple zinc–copper cell, bubbles of hydrogen gas form on the copper as current flows. They cover it, block the liquid, and the voltage drops — often to half within minutes. This is called polarisation. You can revive the cell by lifting the copper out and brushing it, or by letting it rest. The Daniell cell (Method 3) cures polarisation completely and gives a steady 1.1 V for weeks.

What you need

Item Amount Notes
Zinc 200 g for a small pile; 1–2 kg for a bank of Daniell cells See Zinc and Brass — the hardest part
Copper Same area as the zinc, thinner is fine (0.5–1 mm sheet) Copper Smelting
Salt A cupful Salt
Vinegar Optional, instead of brine Fermentation
Cloth, leather or thick paper Discs or strips to hold the electrolyte Spinning and Weaving Cloth, Hides and Leather, Paper
Pots Glazed jars, or wooden cups sealed with wax or pitch Pottery, Tar, Pitch and Glue
Unglazed pots For Daniell cells: small, low-fired, porous Pottery
Copper sulfate (blue vitriol) For Daniell cells, about 0.5 kg See below
Copper wire A few metres, to connect cells Copper Wire

Where to find it

Zinc is the real obstacle. Zinc ores are common — usually found with lead ores in limestone country (see Finding and Identifying Ores) — but zinc metal is hard to make. The temperature needed to free it from its ore (over 1,000 °C) is higher than the temperature at which zinc boils (907 °C). So in an ordinary furnace the zinc escapes as vapour and burns back to white powder in the air. It must be made in a closed clay retort and its vapour caught in a cool condenser. This is explained in Zinc and Brass. Expect it to be a project of its own. Every gram is precious; keep scraps for remelting.

If you cannot make zinc, use iron as the negative plate with copper or carbon as the positive. You will need about three times as many cells for the same voltage, but iron is easy (Iron (the Bloomery)).

Copper comes from Copper Smelting smelting. For the positive plate, carbon also works: a dense, hard piece of coke or charcoal that rings when tapped, or natural graphite (the soft, black, greasy mineral that marks paper). Ordinary soft charcoal conducts poorly; it must be dense.

Brine is salt dissolved in water — about 1 part salt to 5 parts water by weight, or a heaped handful per mug. Vinegar works about as well. Dilute sulfuric acid gives more current than either (Sulfuric Acid); mix about 1 part acid into 15 parts water.

Copper sulfate (blue vitriol) is a bright blue crystal. Make it like this: heat scraps of copper red-hot in an open fire for an hour so that they are covered in black scale; knock off the scale and dissolve it in warm dilute sulfuric acid, stirring; the liquid turns deep blue. Let the water evaporate slowly in a shallow pot and blue crystals grow. In old copper mining country, blue water seeping from mine workings and blue crusts on the rocks around them are natural copper sulfate.

Method 1: Volta's pile

The simplest battery, and the one Volta built first.

ONE CELL, ENLARGED next cell's zinc Copper Wet cloth Zinc ONE CELL each cell gives about 0.8–0.9 V + end top copper − end bottom zinc Stone weight presses the discs Frame waxed sticks 10 cells ≈ 8–9 volts
Fig. 2 A voltaic pile in cross-section. Zinc, cloth soaked in brine, and copper are stacked in the same order again and again. Each zinc–cloth–copper layer is one cell; the cells add up in series.
  1. Cut discs. Make 10–20 discs each of zinc and copper, about 4 cm across (the size of a large coin). Zinc 1–2 mm thick, copper 0.5–1 mm. Clean both faces bright by scouring with sand.

  2. Cut separators. Cut the same number of discs from cloth (two or three layers), soft leather or thick paper, about 3 mm smaller across than the metal discs.

  3. Soak the separators in brine (or vinegar). Squeeze them until they no longer drip. Too wet, and brine runs down the outside of the pile and shorts the cells together.

  4. Build a frame. Set three straight sticks or glass rods upright in a wooden base, in a triangle just wide enough to hold the discs. Coat any wood with wax so that it does not soak up brine.

  5. Stack in a fixed order, starting at the bottom:

    • zinc → wet cloth → copper → zinc → wet cloth → copper → zinc → …
    • finish with a copper disc on top.

    Each copper disc sits directly on the next zinc disc, metal to metal. Never change the order partway up.

  6. Attach wires. Slip a wire under the bottom zinc (this is the − end) and another on top of the top copper (the + end). A small flat stone on top presses the discs together.

  7. Test (see How to tell it worked). Expect about 0.8–0.9 V per cell: 10 cells about 8 V, 20 cells about 16 V.

A pile gives only a small current — thousandths to hundredths of an amp — because the wet cloths are thin and resist the flow. It is ideal for tests, for a sensitive detector and for a The Telegraph over a short line, but it will not run an electromagnet strongly. It also dries out within a day or two. Take it apart after use, wash the discs, and scour off any white crust from the zinc.

Tip Solder pairs. Solder or rivet each copper disc to a zinc disc face to face. Each "couple" then goes in as one piece, so you cannot get the order wrong, and the contact between them is perfect.

Method 2: The cup battery (crown of cups)

For more current, use bigger plates in pots of liquid.

  1. Set out a row of glazed pots or waxed wooden cups, each holding about half a litre.
  2. Fill each with brine, vinegar, or dilute sulfuric acid (strongest).
  3. Make pairs: a strip of zinc and a strip of copper, each about 5 cm wide and 12 cm long, joined at the top by a short copper wire or a bent strip so that they form an upside-down U.
  4. Hang the pairs over the rims so that the zinc of each pair dips in one pot and its copper in the next pot. In the first pot put a lone copper strip with a wire (+); in the last pot, a lone zinc strip with a wire (−). The zinc and copper in the same pot must not touch.
  5. Each pot is one cell. Ten pots give about 9 V, and much more current than a pile — a good fraction of an amp in acid, for a few minutes, before polarisation sets in.
  6. Lift the plates out when you are not using them. Zinc slowly dissolves in the liquid even with nothing connected.

To get more current from the same pots, use wider plates or put two zinc plates in each pot, one on each side of the copper, joined together.

Method 3: The Daniell cell — steady power

John Frederic Daniell's cell (1836) keeps the copper plate clean of hydrogen by standing it in copper sulfate. Instead of hydrogen, pure copper is laid down on the copper plate. It gives a steady 1.1 V that hardly sags, and it lasts for weeks. It powered the world's telegraphs for half a century.

− + Zinc bar (−) slowly dissolves Porous pot unglazed, lightly fired; soaked in water first Salt water or very weak acid Copper sheet (+) rolled into a cylinder round the porous pot Spare crystals in a cloth bag Copper sulfate saturated, deep blue; fades as it is used Jar glazed pottery or glass steady 1.1 volts
Fig. 3 The Daniell cell. A porous unglazed pot separates the zinc in salt water from the copper in blue copper sulfate. Electricity flows through the damp pot wall, but the two liquids mix only slowly.
  1. Outer jar: a glazed pot or glass jar about 15 cm across and 20 cm tall.
  2. Copper: a sheet of copper about 15 × 30 cm, rolled into a cylinder that stands inside the jar against its wall. Attach a copper wire, well above the liquid line.
  3. Porous pot: a small unglazed, lightly fired (biscuit) clay pot about 7 cm across and 18 cm tall, stood inside the copper cylinder. Soak it in water for an hour first. It must be porous enough to let water seep through slowly, but not leak freely.
  4. Zinc: a thick bar or rolled sheet of zinc, 2–3 cm across, standing in the porous pot, with a wire attached at the top.
  5. Fill the porous pot with brine or very dilute sulfuric acid (1 part in 20), up to 3 cm from the top.
  6. Fill the outer jar with saturated copper sulfate solution — as much blue vitriol as will dissolve in warm water — to the same level. Drop a handful of extra crystals into the outer jar, on a shelf or in a cloth bag hanging just below the surface, to keep it strong.
  7. The copper wire is the + terminal, the zinc wire the −. Expect 1.1 V, very steady, and a current of up to about half an amp into a thick, short wire.

Looking after it. Every amp that flows for an hour dissolves about 1.2 g of zinc and uses up about 4.7 g of copper sulfate crystals; the copper sulfate shows this by fading from deep blue to pale. Add crystals as it pales. Keep the cell covered to slow evaporation. When the zinc side becomes thick with white zinc salts, pour off half of it and top up with water. When not in use for weeks, take the porous pot out and keep it in water, or the copper slowly creeps through and coats the zinc.

The gravity cell (no porous pot)

If you cannot make a good porous pot, use the gravity cell that American and European telegraph offices used from the 1860s. Lay a flat copper plate (or a "crowfoot" of copper strips) on the bottom of a jar, with an insulated wire leading up out of the jar. Cover it with copper sulfate crystals and fill with water. Hang a heavy zinc casting near the top of the jar. Join the two wires together for a few hours when the cell is new. A layer of clear zinc solution then forms above the heavy blue copper sulfate solution, and the two stay apart by their weight alone — as long as the cell is never shaken or moved, and is used a little every day. It gives about 1 V, and lasts for months with occasional topping up.

How to tell it worked

You do not need a meter. In order of sensitivity:

  1. The compass galvanoscope. Wind 20–30 turns of insulated Copper Wire around a small box or bowl, lay a compass or a floating needle inside, and turn the whole thing so the needle lies along the turns of wire. Connect your cell to the two ends. The needle swings sideways; reverse the connections and it swings the other way. Even one small cell moves it clearly. More swing means more current. (How to build a proper one is in The Electromagnet; calibrated meters are in Measuring Electricity.)
  2. The tongue test — for one or two cells only. Touch both wires to the tip of your tongue, 1 cm apart. A working cell gives a sour, metallic tingle. This is how Volta and others first checked their cells. Never do this with more than two or three cells, and never with any battery or generator whose voltage you do not know.
  3. The wet-finger test. With a pile of 15–30 cells, dip one finger of each hand in salt water and touch the two end wires. You feel a tingle or a weak jolt — that is about 15–25 V. Do not go higher.
  4. Bubbles. Put two wires from a battery of three or more zinc–copper cells (or two Daniell cells, 2.2 V) into a cup of salt water, 1–2 cm apart. Fine bubbles stream from the wire joined to the zinc end: that is hydrogen gas, and it proves current is flowing. This is Electrolysis — the discovery that came weeks after Volta's.
  5. A spark. With a large cup battery or several Daniell cells, scrape the end of one wire along a file joined to the other. Small sparks appear.

Note Troubleshooting. No voltage at all → a disc is in the wrong order, two metals of the same kind are touching across a cloth, or a wire is not touching bare, clean metal. Scrape every contact bright. Works for a minute, then fades → polarisation. Brush the copper, let it rest, or move to a Daniell cell. Pile is wet on the outside and gives little → brine is running down and shorting the cells. Squeeze the cloths drier; use smaller separators. Zinc vanishes even when unused → impure zinc dissolves by itself. Lift plates out of the liquid between uses. Daniell cell gives under 1 V and the zinc is coated with copper → the porous pot is too porous or cracked. Fire a new one slightly harder.

Dangers

Danger Acid. Dilute sulfuric acid burns skin and eyes and eats cloth. Always pour acid slowly into water, never water into acid — water added to strong acid boils instantly and spits acid. Wear eye protection. Keep a bucket of water nearby, and wash any splash off at once with lots of water for 15 minutes. See Sulfuric Acid.

Danger Hydrogen explodes. Cells with acid give off hydrogen gas. In a closed box or cupboard it can build up and explode from a single spark. Keep batteries in the open air, and never test them with a flame.

  • Copper sulfate is poisonous if swallowed (vomiting, and worse in children) and irritates eyes and skin. Label its pots clearly, keep it away from food and animals, and wash your hands after handling it.
  • Shocks. A few cells are harmless. But voltages add up: a pile or bank of a hundred cells (about 100 V) can give a dangerous shock through wet skin. Above about 50 V, treat a battery with the respect you would give a live wire. Never let current pass from one hand to the other across your chest.
  • Short circuits and heat. A large cup or Daniell battery joined by a short thick wire can heat the wire enough to burn your fingers or char the insulation. Do not leave batteries connected and unattended.
  • Melting zinc gives off white fumes of zinc oxide that cause "metal fume fever" — a day of fever and shivering. Melt it outdoors, upwind (see Zinc and Brass).

Going further

  • Rechargeable batteries. Two lead plates in dilute sulfuric acid, charged from a The Generator, form a lead–acid battery (Gaston Planté, 1859) that can be charged and used again hundreds of times. See The Rechargeable Battery.
  • Dry cells. A zinc can with a damp paste instead of a liquid, carried in a pocket: see Dry Cells and Electric Torches.
  • Electrolysis. With a battery you can split water, salt and molten salts, plate metals, and refine copper: see Electrolysis.
  • Electromagnets and telegraphs are the first great use of battery current: see The Electromagnet and The Telegraph.

How it was first done

In the 1780s the Italian anatomist Luigi Galvani noticed that the legs of a dead frog twitched when touched by two different metals at once. He believed the electricity came from the frog ("animal electricity"). Alessandro Volta, a physicist at Pavia, disagreed: he thought the two metals were the source, and the frog's leg only a very sensitive detector. To prove it, he stacked discs of zinc and copper (or silver) with cardboard soaked in brine between them, and found he could get a steady current with no animal at all. He described his pile in a letter to the Royal Society in London dated 20 March 1800.

The news spread fast. In May 1800 William Nicholson and Anthony Carlisle in London used a pile to split water into hydrogen and oxygen. By 1807–1808 Humphry Davy, using large batteries of hundreds of cells, had discovered sodium, potassium, calcium and other elements. In 1836 John Frederic Daniell in London invented his steady two-liquid cell, and the telegraph networks of the 1840s–1870s ran on Daniell and gravity cells by the thousand. The unit of electrical push, the volt, is named after Volta.

Source: content/entries/electricity/battery.md