◆ Rebuild

Part 15 · Knowledge and Science

Pens, Nibs and Writing Instruments

How to make the whole family of writing tools beyond the cut quill — penholders and pressed steel nibs, inkwells that do not spill, the fountain pen and its feed, the ballpoint in outline, coloured pencils and better crayons, rubber erasers and pencil sharpeners — and how to tell a good one from a bad one.

Difficulty
●●●●●
Time
Minutes for a reed or quill; a day to make a penholder and a few dozen nibs by hand; a week for a fountain pen with a lathe; an afternoon for crayons, erasers or a sharpener
Steps from zero
14 prerequisites →

You need first

InkSteel

This unlocks

—
The full path from nothing — 14 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Ink
  11. Bellows
  12. Iron (the Bloomery)
  13. Blacksmithing
  14. Steel
  15. Pens, Nibs and Writing Instruments

Do them roughly in this order. See it on the tech tree →

Why it matters

A cut quill writes beautifully, but it softens after a page or two and must be re-cut every day by someone who knows how. A steel nib costs a few seconds of machine work, writes for weeks, and is the same for every pupil. When Birmingham factories began pressing steel pens by the million in the 1830s, cheap writing — and with it mass schooling, clerks, letters and records — spread across the world.

This chapter covers what comes after the basic pens of Ink and the pencils of Pencils and Chalk: dip pens with steel nibs, inkwells, the fountain pen, the ballpoint in outline, coloured pencils, better crayons, erasers and pencil sharpeners. They serve Teaching and Schools, Libraries and Preserving Knowledge, Technical Drawing, bookkeeping and the post.

How it works

Every pen is a controlled leak. Ink is held in a store and drawn out a little at a time by capillary action — the pull that makes water creep into a narrow gap. The narrower the gap, the stronger the pull.

  • In a nib, the gap is the slit between two springy halves called tines. When the tip touches paper, the paper's fibres pull harder than the slit and ink flows. Pressing spreads the tines and thickens the line.
  • The breather hole at the top of the slit stops cracks running up the nib and makes the tines flex evenly.
  • A fountain pen has a sealed store. Ink cannot leave a sealed bottle unless air gets in, so the feed under the nib lets ink run down and air bubble up.

Pencils, crayons and erasers work by friction: paper acts as a fine file. An eraser is a solid that pencil flakes stick to better than they stick to paper.

What you need

Item For Notes
High-carbon steel, 100 g About 200–250 nibs, allowing for offcuts Steel, rolled thin as in Sheet Metal and Rolling
Punches, small anvil, files, fine stones, iron box, oil Nibs Blacksmithing, Files and Saws, Abrasives and Grinding Stones
Ebonite (hard rubber) rod and a lathe Fountain pen Rubber, The Lathe
Raw rubber, sulfur, plant oil Erasers
Wax, pigments, white clay, soapstone Crayons, coloured pencils Pigments, Paints and Varnish
Glass or glazed stoneware Inkwells Glass, Glazes

Quill and reed pens

How to cut both — scoop, slit, shoulders, square tip — is in Ink. Here is how to choose and judge them.

Reed pen

Pick reed stems that are dry, pale and hard — a fingernail should not dent the skin. Use an outside diameter of 7–12 mm, length about 20 cm, a slit of 5–8 mm (reed is stiff; a longer slit gives spring), and a nib 1.5–2 mm wide for writing or 3–6 mm for signs. For Arabic and Persian scripts the tip is cut on a slant of about 30°. Split bamboo makes the same pen. A bad reed pen has fibres sticking out of the tip that drag a hairy line.

Quill pen

Use the five outermost wing feathers of a goose (standard), swan (longest-lasting) or crow (finest lines). Barrel 6–8 mm across, cut to 18–20 cm; slit 6–10 mm; nib 1–2 mm wide. Cure it in hot sand first (Ink): it holds its edge two or three times as long.

Good or bad (both): look at the tip end-on against the light — the two halves must be level and the cut square. A good pen makes a hair-thin sideways stroke and a full-width downstroke, writes 5–10 words per dip, and does not spit. Fat, blurred lines mean the tip has softened: re-cut it.

The dip pen and steel nib

A dip pen is a penholder (handle) and a removable nib: a curved piece of springy steel like a tiny half-tube with a pointed, slit end. When it wears out after a few weeks you change only the nib.

35–40 mm 8–9 mm slit 9–12 mm Tip and tines two springy halves Slit sheared, dead centre Breather hole 1.5–2 mm Side cut Shank Shoulder ground thin behind tip 1 Cut blank from 0.2 mm annealed steel strip 2 Pierce hole punch on end grain; make side cuts 3 Raise (end view) rod struck into a groove curls blank into half-tube 4 Harden, temper, slit temper to brown-blue, shear slit, grind, polish
Fig. 1 A steel nib and how it is made. A flat blank is punched from thin steel, the breather hole pierced, the blank curved in a die, hardened and tempered, then slit from the tip to the hole and ground smooth.

Key sizes

Part Size
Steel thickness 0.2–0.25 mm (school pens); 0.15 mm for flexible drawing nibs
Blank length 35–40 mm
Width at the shank (the end held by the holder) 8–9 mm, curved to a radius of about 4 mm
Breather hole 1.5–2 mm across, 9–12 mm from the tip
Slit From the tip to the breather hole, as thin as you can make it
Penholder 15–18 cm long, 9–11 mm thick at the grip

Making nibs by hand

This gives a few dozen nibs a day.

  1. Strip. Hammer or roll high-carbon steel (about 1% carbon; bushy, branching sparks in the spark test of Steel) to 0.2–0.25 mm thick. A small rolling mill (Sheet Metal and Rolling) gives the even thickness that makes nibs write alike. Old clock springs are ready-made strip.
  2. Anneal. Heat to dull red (about 700 °C) and cool slowly in wood ash so it is soft.
  3. Cut blanks round a brass template — a pointed shape 38 mm long and 9 mm wide at the back — with small shears, and file the edges smooth.
  4. Pierce the breather hole with a 1.5–2 mm punch, the blank lying on end-grain hardwood. Two short side cuts toward the hole make the point more flexible.
  5. Raise. Lay the blank across a groove filed in a steel block, set an 8 mm polished steel rod along it and strike the rod once. The blank curls into a half-tube; both sides must curve equally.
  6. Harden. Pack the nibs in charcoal dust in a lidded iron box, heat to cherry red, about 800 °C, hold 10 minutes, and tip everything into oil. They are now glass-hard.
  7. Scour off the scale by tumbling in a jar of wet sand for an hour.
  8. Temper. Stir them in a pan of dry sand over a gentle fire until they pass straw and reach brown going to blue (about 280–300 °C), then tip them onto a cold stone. That is a spring temper.
  9. Grind the top of the point, just behind the tip, across a fine stone, so the tines are thin enough to flex.
  10. Slit — the step that makes or breaks the pen. Set the nib on the sharp square edge of a hardened steel block. Lay a thin, very sharp hardened chisel exactly on the centre line from the tip to the breather hole and press down in one firm stroke. It must shear the steel cleanly, like scissors.
  11. Point the tip by rubbing in small circles on a fine stone, then on leather with tripoli, so it glides in every direction. Dip in thin shellac varnish against rust.

The industrial version

In a factory each step is a separate machine and worker, as in Needles and Pins. A fly press (a screw press with a heavy swinging arm) with a hardened punch and die stamps blanks as fast as the operator feeds strip; other presses pierce, raise and stamp a maker's mark; a slitting press with two hardened blades shears the slit. Hardening is done by the thousand in iron boxes, tempering in a slowly turning iron drum over a fire. Ten workers make tens of thousands of nibs a day. The dies need Machine Tools and careful gauging (Precision and Interchangeable Parts).

The penholder

The simplest holder is a reed or stick with a saw cut 12 mm deep in one end; the nib is pushed in and wedged by its own spring. Better: a turned hardwood holder with a tin-plate sleeve round its tip and a thin sprung metal tongue inside, gripping the nib between them. Keep the grip at least 9 mm thick; thin holders cramp the hand.

Good or bad

  • Tines touch at rest and are the same length (check with a magnifying glass, Lenses); the slit is dead centre and runs right into the breather hole.
  • It springs back after the tines are pressed open to twice the line width.
  • It writes a line of 8–15 words per dip with no scratching on upstrokes or sideways strokes.
  • Rusted nibs, uneven tines, or a slit that stops short of the hole: throw away.

Tip Iron-gall ink (Ink) is acid and slowly eats steel. Wipe nibs on a cloth pen wiper after use and they last three or four times longer. Wash new nibs with soap before use: the film of hardening oil stops ink wetting them.

The inkwell

An inkwell must hold ink without tipping, drying out or letting the pen dip too deep.

  • Material: glass, or stoneware glazed inside. Unglazed clay soaks up ink; iron-gall ink corrodes metal.
  • Shape: squat and heavy — about 7 cm wide and 4–5 cm tall — with a mouth no wider than 2.5–3 cm, and a lid or cork.
  • Depth: the nib should go in only to its breather hole, about 1 cm.
  • Non-spill: mould or glue a cone into the mouth, pointing down inside, its open tip within 1.5 cm of the bottom. Knocked over, the ink lies in the corner round the cone and cannot reach the hole.
  • School desk well: a small glazed pot 4 cm across with a rim, dropped into a hole bored in the desk top.
Non-spill inkwell Hand pencil sharpener Cone open tip 1.5 cm above the floor Ink Wide heavy base 7 cm wide, 4–5 cm tall knocked over: ink stays in the corner Blade edge 0.1–0.3 mm in Screw Shaving 8 mm mouth Cone ~20° Block hardwood or brass, 25 mm long turn
Fig. 2 Two tools in section. Left: a non-spill inkwell — the inward cone keeps the ink in when it is knocked over. Right: a hand pencil sharpener, with the blade lying along one side of a cone bored into the block.

The fountain pen

A fountain pen carries several days' ink in its barrel. The simplest kind, the eyedropper pen, is filled with a dropper after unscrewing the front.

Barrel ebonite, 8 mm bore Ink 3–4 ml, thin, no gum Thread smeared with beeswax Section Fins catch overflow Feed slot 0.2–0.4 mm wide;ink down, air up Nib Breather hole Air bubbles in replace the ink used Cap with inner cap seals nib from air
Fig. 3 An eyedropper fountain pen in section. Ink runs down the slot in the feed to the nib by capillary action, and air bubbles up the same slot into the barrel to replace it. The fins under the nib catch overflow when the barrel warms.

Parts and sizes

Part Material Size
Barrel Ebonite (hard rubber), closed at the back 12–13 mm outside, 8 mm bore, 110 mm long; holds about 3–4 ml
Section (the grip) Ebonite Threaded into the barrel; bored 5 mm through
Feed Ebonite rod 5 mm, filed flat on top, with a slot 0.2–0.4 mm wide, 2 mm deep
Nib Steel, or gold with a hard tip Curved to fit snugly over the feed, breather hole over the slot
Cap Ebonite With an inner cap that seals against the section so the nib does not dry out

Ebonite — rubber cured with 35–50 parts sulfur per 100 (Rubber) — is the right material: ink does not attack it and it turns, drills and threads well. Hardwood swells and leaks.

Making one

  1. Barrel. On the The Lathe, turn the rod round, drill an 8 mm hole 100 mm deep, and cut an inside thread at the open end (Screws, Nuts and Bolts).
  2. Section. Turn a short piece with a matching outside thread and a tapered grip; drill it through at 5 mm.
  3. Feed. File a 5 mm ebonite rod flat along one side. Saw the slot along the flat with the thinnest saw you have (a jeweller's saw, or clock spring with teeth filed on). File 4–6 thin fins across the underside.
  4. Fit the nib on the flat of the feed and push both tightly into the section, the tip standing 12–15 mm out.
  5. Fill. Smear the thread with beeswax, fill the barrel two-thirds with ink from a dropper, and screw it together.

Good or bad: it starts at the first touch after a day capped; it does not blot when a warm hand expands the air in the barrel (if it does, add fins or narrow the slot); the line does not fade down a long page (if it does, air cannot get in — widen the slot a little).

Ink matters. Carbon and gummy inks clog the slot within hours. Use a thin, filtered ink with no gum — iron-gall ink with half the usual iron, or a dye ink (Dyes and Mordants, Coal Tar Chemicals) — and flush the pen with water every week or two. Steel nibs rust in fountain pens; the best have gold nibs (Gold and Silver) tipped with a welded bead of osmium–iridium, a hard native alloy found as heavy grains with platinum (Palladium, Rhodium and Iridium).

The ballpoint pen in outline

A ballpoint pen has a steel ball of 0.7–1.0 mm held in a brass socket at the end of a narrow tube of ink. The socket's lip is pressed in over the ball so about a third sticks out; as the ball rolls it carries a film of ink from the tube, and air follows the ink in at the open back. One pen writes 2–3 km of line.

It is hard to make. The ball must be round to about a thousandth of a millimetre (Making Ball and Roller Bearings); the socket must hold it with a gap of a few thousandths — looser and it blobs, tighter and it skips; and the ink is a honey-thick paste of dye in an oily liquid with resin that dries in seconds on paper but never in the tube. It is a goal for a workshop with precision grinding and Machine Tools. Until then, dip pens, fountain pens and pencils do everything it does.

Coloured pencils

A coloured pencil has a core of pigment, wax and clay, cased in wood. Unlike graphite leads, the cores are never fired — heat would burn the wax and spoil most colours.

  1. Mix by dry weight: 25 parts pigment (ochres, burnt umber, soot, chalk, Egyptian blue — see Pigments, Paints and Varnish), 35 parts kaolin or other fine white clay, 15 parts powdered soapstone (for glide) and 5 parts gum arabic dissolved in a little hot water.
  2. Knead and grind on a stone slab for half an hour, then stir in 20 parts melted beeswax or tallow while the slab is warm.
  3. Roll or extrude rods 3.5 mm thick, as for pencil leads in Pencils and Chalk.
  4. Dry straight in grooved boards for 3 days.
  5. Soak in melted wax at about 80 °C for half an hour; wipe.
  6. Case in wood as for graphite pencils, but make the grooves deeper to take the thicker core, and glue the core along its whole length — the soft core breaks easily if it can move. Finished diameter about 8 mm.

Good or bad: a good coloured pencil lays an even, strong colour with light pressure, does not scratch, and can be sharpened to a point that survives a few lines. A crumbly core has too little wax or gum; a pale, greasy one too much wax.

Crayons

Pencils and Chalk makes crayons from 2–3 parts beeswax to 1 part pigment. Two improvements:

  • Harder, cleaner crayons: 65 parts paraffin wax (Petroleum and Refining), 10 parts stearin (the hard fat acid of candles, Lamps and Candles) and 25 parts pigment. They do not soften on a warm day or feel greasy.
  • A proper mould: a row of 9 mm holes 95 mm deep drilled in a brass block, or in a split hardwood block clamped together. Grease, pour, cool 20 minutes (stand brass in cold water), push the crayons out with a rod, and wrap each in paper with starch paste.

A good crayon is 9–11 mm thick and about 9 cm long, lays bright colour without crumbling, and does not snap under a child's grip.

Warning Never use lead white, red lead, vermilion (cinnabar), orpiment or chrome yellow in crayons, coloured pencils or anything children handle. Children chew them. Use earths, soot, chalk and plant colours.

Erasers

Bread and soft raw rubber both rub out pencil (Pencils and Chalk). Raw rubber turns sticky in summer and hard in winter. A proper eraser is a lightly vulcanised rubber softened with factice.

  1. Make factice. Heat 100 parts rapeseed or linseed oil to about 150 °C (a drop of water flicked on it spits instantly), then stir in 15–20 parts powdered sulfur a little at a time. Hold it there, outdoors, until it thickens to a brown, crumbly, rubbery mass — about an hour. Cool and crumble it.
  2. Mix on the warm slab, as in Rubber: 100 parts masticated rubber, 100 parts factice, 50 parts chalk, 3 parts sulfur, 2 parts lime. For an ink eraser add 50 parts fine pumice — it grinds away the top fibres of the paper with the ink.
  3. Press into a slab 10 mm thick and cure buried in sand at 130–150 °C for about an hour.
  4. Cut into blocks about 40 × 20 × 10 mm. Cut rods of 6 mm for pencil-top erasers and crimp them into a short tin-plate ferrule on the end of the pencil.

A kneaded eraser for drawing is raw rubber worked with an equal weight of chalk and a few drops of oil.

Good or bad: a good eraser lifts a pencil line in two or three strokes, its crumbs roll up grey, and it does not smear or tear the paper. Smearing means too little factice or filler; skidding without lifting means over-cured or old.

Pencil sharpeners

A sharp knife sharpens any pencil. A pencil sharpener does it faster, evenly and with no skill: a block with a cone bored into it and a blade screwed across a window in one side of the cone. Turning the pencil shaves off a thin ribbon of wood and lead.

Part Size
Block Hardwood, brass or cast metal, about 25 × 15 × 15 mm
Cone 8 mm at the mouth (pencil diameter), included angle about 20° — 18–24° works
Blade Hardened steel 0.5–1 mm thick, 15 × 25 mm, honed sharp
Blade setting Edge lies along a line of the cone and stands in by only 0.1–0.3 mm
  1. Make a cone reamer. File a steel rod into a cone of the same angle, then file one half away so it is shaped like a letter D in section. Harden and temper it to straw (Steel).
  2. Bore an 8 mm hole 25 mm into the block, then twist the reamer in until the cone's mouth is 8 mm across.
  3. Cut the window. Saw and file away one side of the block until you just break into the cone along its whole length.
  4. Fit the blade across the window with a small screw, its edge parallel to the cone's side. Adjust until it takes a thin shaving.

Good or bad: the point comes out centred and the lead does not snap. Snapping means the cone angle is too narrow or the blade blunt; a stubby point, too wide an angle. A crank sharpener, with two spiral cutters orbiting the pencil, is faster for schools but needs Gears.

How to tell it worked

  • Nib test. Upstrokes, downstrokes and circles: no scratch, splutter or blot, and the downstroke swells when pressed.
  • Fountain pen test. Capped overnight nib up, then nib down, it starts at once both times and does not drip held a minute in a warm hand.
  • Inkwell test. Knock the non-spill well over on paper: no more than a drop comes out.
  • Eraser and sharpener test. Rub out a pencil line and write over the spot in ink without feathering. Sharpen ten pencils without breaking a point.

Note Troubleshooting. Nib snaps when pressed → still too hard; re-temper to blue. Nib stays bent → over-tempered, or never hardened. Ink floods down the slit → slit too wide or tines bent apart; squeeze together and re-point. Fountain pen writes a few words then stops → air cannot get in; widen or clean the feed slot. Coloured cores break inside the pencil → glue the whole length. Crayons hollow in the middle → poured too hot; pour just above melting and top up.

Dangers

  • Knives and punches. Cut away from the hand holding the work; keep fingers off the punch face.
  • Hardening oil can catch fire when red-hot steel goes in. Use a deep bucket with a lid at hand; never water on an oil fire.

Danger Hot oil and sulfur. Making factice or ebonite gives off choking, poisonous sulfur gases. Work outdoors, upwind, with a lid ready to smother flames. Hot oil and molten sulfur cause deep burns; keep children away.

  • Pigments. See the warning above. Wash hands after grinding any pigment.

What this unlocks

Cheap, uniform pens let a whole village learn to write (Teaching and Schools), keep accounts (Money, Trade and Record-keeping, Records, Bookkeeping and Accounts), run a The Post and fill exercise books. Fine drawing nibs serve Technical Drawing and Maps and Mapmaking. The nib press is a first exercise in mass production with dies, the skill behind coins, buttons and Precision and Interchangeable Parts. For copies, go on to the The Typewriter, Duplicating: Carbon Paper, Hectograph and Stencil and Printing.

How it was first done

Egyptian scribes wrote with rush brushes and later cut reeds; the reed pen (kalamos, qalam) served the Greek, Roman and Islamic worlds. The quill came into use in Europe around the 6th century AD and ruled for some 1,300 years. Metal pens were made by hand in small numbers from Roman times; in the 1820s–1830s Birmingham makers such as John Mitchell, Josiah Mason and Joseph Gillott began stamping steel nibs with presses, and by the 1850s the city made a large share of the world's pens. Petrache Poenaru patented a fountain pen in Paris in 1827, but blotting was only tamed by feeds like Lewis Waterman's of 1884. John Loud patented a ball pen for marking leather in 1888; the practical ballpoint came from László Bíró, a Hungarian working in Argentina, in the early 1940s. Rubber was found to rub out pencil around 1770 (Joseph Priestley wrote about it; Edward Nairne sold it), and Hymen Lipman patented a pencil with an eraser in 1858. Bernard Lassimonne patented a pencil sharpener in France in 1828. Boxed wax crayons became common around 1900.

Source: content/entries/knowledge/pens-and-pencils.md