◆ Rebuild

Part 15 · Knowledge and Science

Photography

Let light draw its own pictures on paper or glass coated with silver salts. A lens in a dark box, silver from the cupel, salt, seaweed, oak galls and a little sulfur give you exact records of faces, places, plants, stars and whole pages of books.

Difficulty
●●●●●
Time
A day to build a camera; a week to make the chemicals; an afternoon per batch of paper; minutes to hours per picture
Steps from zero
20 prerequisites →

You need first

LensesGold and SilverLaboratory Glassware

This unlocks

Photographic Film BaseMaking Photographic Papers and PlatesIntegrated CircuitsMaking MicrochipsBlueprints and CyanotypesCinema: Film Cameras and ProjectorsColour PhotographyThe Darkroom and the EnlargerPlatinum, Salt and Iron-Salt PrintsMicrofilm and Document StorageCopying Documents and Xerography
The full path from nothing — 20 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. The Kiln
  9. Pottery
  10. Charcoal
  11. Hides and Leather
  12. Lime
  13. Lye and Potash
  14. Glass
  15. Bellows
  16. Copper Smelting
  17. Lead
  18. Laboratory Glassware
  19. Lenses
  20. Gold and Silver
  21. Photography

Do them roughly in this order. See it on the tech tree →

Why it matters

A photograph is drawn by the light itself: the exact shape of a leaf, a crack in a bridge, a wound before and after treatment, a face, a star, every word on a page.

  • Records that cannot be argued with — boundaries, buildings, injuries, a machine before it failed.
  • Copies of documents. One exposure copies a whole page, drawings included, and can shrink it so that a book fits on a few glass plates — a powerful way to keep knowledge alive (see Libraries and Preserving Knowledge).
  • Science. Faint stars gathered over an hour through a The Telescope (Astronomy), bacteria under the The Microscope, bones seen by X-Rays.

Photography rests on one fact from Silver Nitrate and Silver Salts: silver salts darken in light. Everything else is a way to make that darkening faster, stop it at the right moment, and make it permanent.

How it works

  1. The camera. A lens at one end of a dark box makes a small, upside-down image on the back wall.
  2. The sensitive layer. Silver chloride, bromide or iodide, made in the pores of paper or in a film of gelatin on glass.
  3. Printing out or developing. In strong light, silver chloride darkens visibly on its own (printing out) — fine for copying in sunshine, far too slow in a camera. A short exposure instead leaves an invisible latent image, and a developer (gallic acid or pyrogallol, from oak galls) turns the touched crystals, and only those, into black silver. Development multiplies the effect of light hundreds of times.
  4. Fixing. A fixer (sodium thiosulfate, "hypo") dissolves the unexposed silver salt away. Washing then removes the fixer.
  5. Negative and positive. The camera picture is a negative: bright sky black, dark trees clear. Laid on fresh paper in the sun, it gives a positive. One negative makes any number of prints.
The scene light from every point Stop hole 10–20 mm Lens f = 150–300 mm Two boxes blackened inside Ground glass what you see on it: the scene upside down slide to focus lens to screen: about the focal length (more for near things)
Fig. 1 A box camera in cross-section. Rays from the top of the tree cross at the lens and land at the bottom of the screen, so the image is upside down. Slide the back box until the image is sharp, then replace the screen with the plate holder.

What you need

Item Amount Notes
Lens 150–300 mm focal length, 25–40 mm across See Lenses
Two boxes, one sliding inside the other Thin wood, blackened inside with soot in glue
Ground-glass screen, dark cloth Glass
Silver 10–20 g to start Gold and Silver
Nitric acid About 1.5 ml strong acid per gram of silver Nitric Acid
Salt, potassium iodide, gallic acid, hypo A cup; 20–40 g; 10–20 g; 200–500 g Made below
Gelatin 100 g The clearest hide glue: Glues and Adhesives
Paper Smooth, well-sized rag paper Paper
Dishes, bottles, glass rods, measures Glass or glazed stoneware: Laboratory Glassware
Rain or distilled water Many litres Hard well water spoils silver baths; Distillation
Printing frame Picture frame with a glass front and hinged wooden back
Red safelight Candle or lamp behind ruby glass or 3–4 layers of madder-red cloth

Tip Keep a notebook. Write down every strength, time, temperature and the weather for each exposure. Photography rewards the The Scientific Method more than almost any craft.

Where to find it

  • Silver — native silver, or silver cupelled out of lead ore (Gold and Silver). Old coins and spoons contain copper (see below).
  • Seaweed — brown kelps and wracks on rocky coasts. Their ash is the only common natural source of iodine.
  • Manganese ore — heavy, sooty black, soft, staining fingers black; often with iron ores (Finding and Identifying Ores).
  • Oak galls — as in Ink. Sulfur — yellow crusts at volcanic vents, or made from pyrite (Sulfur).
  • Hide and bone for gelatin, eggs for albumen paper, beeswax to clear paper negatives.

Building the camera

  1. Measure the lens. Focus the sun to the smallest spot; the lens-to-spot distance is the focal length (f). 200 mm is a good start.
  2. Make two boxes. The front one, about 15 × 15 cm across and a little longer than f, holds the lens. The back one slides inside it snugly, so the lens-to-back distance can range from about 0.8 f to 1.5 f. Blacken every inside surface; stray light fogs the picture.
  3. Fit a stop, a black disc with a round hole, just in front of the lens. A simple lens is only sharp across the picture when stopped down. The f-number is focal length ÷ hole diameter: 200 mm with a 15 mm hole is about f/13. Each time you multiply the f-number by 1.4, the exposure doubles.
  4. Ground glass. Rub one pane against another with fine emery and water (Abrasives and Grinding Stones) for 15–20 minutes until evenly frosted. Frame it at the back, frosted side towards the lens.
  5. Plate holders. Shallow frames that put the plate exactly where the frosted surface was, with a light-tight sliding lid (the dark slide).
  6. Shutter. A lens cap. Exposures are seconds or minutes long.

To use: focus under the dark cloth, cap the lens, swap the screen for a loaded holder, pull the slide, uncap for the exposure, cap, close the slide.

No lens? A pinhole works. The sharpest hole is about 0.036 × √f mm: 0.5 mm for f = 200 mm, pierced with a fine needle in thin copper or brass foil and sanded smooth. At about f/400 it is more than 500 times slower than f/16 — usable only with gelatin plates and still scenes.

Making the chemicals

Silver nitrate. Outdoors, put 10 g of silver, cut small, in a glass flask with 15 ml strong nitric acid and 15 ml water, and warm gently in a water bath. It dissolves with brown fumes — stand upwind and well back. Evaporate in a glazed dish until a crust forms at the edge, then cool: colourless, flat crystals grow. Evaporate the leftover liquid again for a second crop. 10 g of silver gives about 15.7 g of silver nitrate. A blue or green liquid means copper: redissolve the crystals in a little hot water and crystallise again until crystals and liquid are colourless. Store in a dark, stoppered bottle.

Potassium iodide. Burn dried brown seaweed to ash (very roughly 1 kg of ash from 20 kg of fresh weed). Soak the ash in hot water, filter and boil down; salt and potash salts crystallise first — rake them out and keep the thick, dark mother liquor. Warm it gently in a flask with a little powdered manganese ore and Sulfuric Acid: violet vapour of iodine rises and condenses in a cold jar as grey-black, shiny crystals. Stir the iodine into water with iron filings to make pale green iron iodide; add potash solution (from wood ash, see Lye and Potash) until no more brown sludge falls; filter and boil down. White cubes of potassium iodide crystallise (Iodine covers this in full).

Gallic acid. Soak 200 g of crushed galls in 1 litre of water for a few days (the tannin of Ink). Then either leave it loosely covered in a warm place for 4–6 weeks while mould works on it, or boil it for a few hours with a cupful of dilute Sulfuric Acid (1 part acid to 10 of water). Either way tannin becomes gallic acid, which barely dissolves in cold water and settles as greyish crystals. Redissolve in the least boiling water, filter through cloth with crushed Charcoal, and cool slowly for pale needles. Pyrogallol, the stronger developer for gelatin plates, comes from heating dry gallic acid in a small retort to about 200–220 °C, just short of charring: it rises as white feathery crystals on the cool neck.

Hypo. Burn Sulfur in a small closed stove and lead the choking fumes through a pipe into a strong solution of Soda Ash and Baking Soda until it stops fizzing; then dissolve the same weight of soda ash again into it. This is sodium sulfite. Add powdered sulfur, about 1 part to 4 of sulfite, and boil for an hour, topping up the water. Filter and boil down: large clear crystals that melt in their own water at about 50 °C. If you have no hypo yet, a saturated salt solution "stabilises" a picture for years, though it slowly changes colour.

Method 1: Salt prints

Silver chloride made inside the paper: too slow for the camera, but perfect for copying leaves, lace or drawings on thin paper, and for printing from negatives.

  1. Salt. Soak sheets for 3 minutes in 20 g of salt per litre of water (2%), with a teaspoon of gelatin. Hang to dry.
  2. Sensitise in dim light: brush one side evenly with silver nitrate, 12 g in 100 ml water. Dry in the dark; use within a day.
  3. Expose in the printing frame in sunshine, the object or negative against the paper. Peep by opening half the hinged back. Print until the image is darker than you want — 5–30 minutes in summer sun, an hour or more in winter. It lightens in the fixer.
  4. Wash until the milky drip stops, fix 10 minutes in hypo (10–15 g in 100 ml water), and wash an hour in changing water. The image is warm reddish-brown.

Albumen paper is sharper and glossier: beat egg white with 2–3% salt, let the froth settle overnight, float the paper on it for a minute, dry, then sensitise as above. Most 19th-century portraits are albumen prints.

Method 2: Paper negatives (calotype)

The first camera process to try; every chemical comes from this chapter.

  1. Iodise. Brush smooth, well-sized paper with silver nitrate (4 g in 100 ml), dry it, then dip it 2 minutes in potassium iodide (6 g in 100 ml). Yellow silver iodide forms. Rinse 30 minutes in water and dry. This paper keeps for months in the dark.
  2. Excite it by candlelight just before use. Make aceto-nitrate (6.5 g silver nitrate, 60 ml water, 10 ml of the strongest distilled vinegar you have — see Fermentation) and a saturated gallic acid solution in cold water (about 1 g in 100 ml). Mix equal parts only at the moment of use — it turns brown and useless within an hour. Brush it on lightly, wait half a minute, blot, and load the paper still slightly damp.
  3. Expose 1–5 minutes in bright sun at about f/15; much longer in shade.
  4. Develop in the dark: brush on more of the mixture and warm the paper gently, well away from a fire. The image appears over 1–10 minutes. Stop when the shadows begin to grey.
  5. Fix 10–15 minutes in hypo (20 g in 100 ml) and wash an hour.
  6. Wax the dry negative: iron beeswax shavings into it between blotting papers. It becomes translucent and prints far more sharply.

Print it as a salt print. Paper fibres make it soft and grainy — fine for portraits, too soft for copying small print.

1. Scene bright sky, dark tree; expose paper or plate in the camera 2. Negative develop, fix, wash; light parts turn black, dark parts stay clear 3. Contact print negative pressed on salt paper under glass, 5–30 minutes of sun 4. Positive wash, fix, wash again; tones the right way round, brown-black One negative can print hundreds of positives.
Fig. 2 From scene to print. The camera makes a negative, in which light things are dark; the negative laid on fresh paper in sunlight makes a positive, the right way round.

Method 3: Gelatin dry plates

Silver bromide in gelatin on glass is hundreds of times faster than the calotype, gives fine detail and keeps for months. This is the plate for X-Rays, Astronomy and document copying.

Bromide comes from bittern, the bitter liquid left after making Salt from seawater. Chlorine (Chlorine and Bleach) passed through bittern frees bromine, which is carried off as vapour and caught at once on wet iron, never collected as the liquid; the iron bromide, treated with potash exactly like iodine above, gives potassium bromide (Bromine and Bromides). Bromine is among the most dangerous substances in this book; read Bromine and Bromides first. Without it, use salt instead of bromide: a slow silver chloride plate that still copies documents well in sunlight.

Clean the glass (for example 9 × 12 cm) with Lye and Potash and chalk, rinse, and coat thinly with gelatin water (1 g in 100 ml, with a pinch of alum) so the emulsion grips. Dry.

The emulsion — red light only from step 2:

  1. Soak 10 g gelatin in 100 ml water for 15 minutes, warm to 50 °C (hot to the hand, not painful), and dissolve 8 g potassium bromide in it.
  2. Dissolve 10 g silver nitrate in 100 ml water at the same temperature.
  3. Stirring hard, pour the silver into the gelatin in a thin stream over about 5 minutes. It turns milky cream.
  4. Ripen at 50–55 °C for 30–60 minutes. Longer gives a faster plate but more fog.
  5. Stir in another 15 g of soaked gelatin, pour into a dish, and let it set somewhere cool for several hours.
  6. Wash: press the jelly through coarse cloth into noodles and soak them in 5–6 changes of cold water over 2–3 hours.
  7. Remelt at 40 °C, strain, and pour about 5 ml per 9 × 12 cm plate, tilting to spread it. Set the plates on a level slab of cold stone, then dry 1–2 days in a dark, dust-free box.

Expose roughly 1–4 seconds at f/16 in daylight — find yours with test strips. Develop 3–6 minutes at about 18–20 °C in 0.3 g pyrogallol, 3 g sodium sulfite and 3 g soda ash in 100 ml water, mixed just before use. Rinse, fix in hypo (20 g in 100 ml) until the creamy colour has gone and as long again, and wash 30–60 minutes.

Test the safelight: lay a coin on an unexposed plate under it for 5 minutes, then develop. If the coin's outline shows, add a layer or move the light further away.

Wet collodion (outline only). From 1851 to about 1880 most photographs were made on glass coated with iodised collodion, dipped in silver nitrate and exposed while wet — exposures of seconds and superb detail. Collodion is nitrocellulose, a close relative of the explosive guncotton, and this book does not describe how to make it (see Early Plastics). Gelatin plates do everything it did, more safely.

How to tell it worked

  • Test strips. Cover a strip with a card and pull the card back in steps — every 30 seconds for paper, every second for plates. Develop. The step where the brightest sky is just black is your exposure. Record it with the weather.
  • A good negative has clear shadows, a dense but not opaque sky, and detail in both when held to the light.
  • Is it washed? A drop of weak silver nitrate (1 g in 100 ml) on a clean margin should stay clear. A yellow-brown spot after a minute means hypo is left — wash longer, or the picture will fade.

Note Troubleshooting. Whole sheet or plate grey → light leak, unsafe safelight or over-ripened emulsion. Look for leaks from inside the camera, under the dark cloth, in sunshine. Image too faint → too short an exposure, or old developer. Mix gallo-nitrate fresh. Brown blotches → dirty glass or dishes, or uneven brushing. Use rain water; wash every vessel. Prints fade or yellow → poor fixing or washing. Emulsion slides off → no gelatin under-coat, or warm wash water. Keep it below 20 °C. Blurred → camera moved, focus slipped, or stop too wide for a simple lens. Use f/16 or smaller.

Dangers

Danger Silver nitrate blackens skin for days and can blind if a crystal or splash reaches the eye. Wear glass eye protection; rinse any splash in the eye with clean water for 15 minutes. It is poisonous to swallow. Lock it away from children.

Danger Fumes kill, sometimes hours later. Silver in nitric acid gives brown nitrogen dioxide, which can fill the lungs with fluid 3–30 hours after you felt fine; anyone who breathed it must rest and be watched for at least a day and a half. Burning sulfur gives choking sulfur dioxide; iodine vapour burns eyes and lungs; chlorine and bromine are deadly, and bromine also burns skin deeply. Work outdoors, upwind, in small quantities, with someone watching from a safe distance.

  • Pyrogallol is a poison that soaks through skin. Handle it with a glass rod, never fingers.
  • Never use the old shortcuts of mercury vapour (the daguerreotype) or cyanide fixer. Both killed photographers.
  • Acids: see Nitric Acid and Sulfuric Acid.

What this unlocks

Photography turns the The Telescope and The Microscope into recording instruments, makes X-Rays useful, and copies Maps and Mapmaking, drawings and books exactly. Pages photographed 10–20 times smaller onto fine-grained plates — the idea of Microfilm and Document Storage — put a library in a box; well-fixed and washed silver on glass, kept cool and dry, should last centuries (Libraries and Preserving Knowledge). Photographic plates record spectra for chemistry and astronomy and later the patterns of Integrated Circuits.

Next steps: gold toning (a very dilute gold chloride bath, from gold dissolved in Nitric Acid mixed with Hydrochloric Acid, makes prints purple-black and longer-lasting); enlarging (a camera run backwards with a lamp behind the negative, The Darkroom and the Enlarger); factory-made printing papers (Making Photographic Papers and Plates); cyanotype "blueprints" made with iron salts instead of silver, for copying drawings cheaply (Blueprints and Cyanotypes); flexible roll film (Photographic Film Base); and Colour Photography.

How it was first done

The Chinese thinker Mozi described the pinhole image around 400 BC, and Ibn al-Haytham explained the camera obscura in Cairo about 1021. In 1717 Johann Heinrich Schulze showed that silver salts darken with light, not heat. Joseph Nicéphore Niépce made the oldest surviving camera photograph, the view from his window at Le Gras in France, in 1826 or 1827, with bitumen on pewter and an exposure of probably many hours. His partner Louis Daguerre announced the daguerreotype, developed in mercury vapour, in 1839. William Henry Fox Talbot made paper negatives from 1835 and patented the calotype, developed with gallic acid, in 1841. John Herschel found in 1819 that hypo dissolves silver salts, proposed it as a fixer in 1839, coined "photography", "negative" and "positive", and invented the cyanotype in 1842 — used by Anna Atkins in 1843 for the first book illustrated with photographs, of seaweeds. Frederick Scott Archer published wet collodion in 1851; Richard Leach Maddox proposed gelatin plates in 1871; and George Eastman's Kodak of 1888 put roll film into everyone's hands.

Source: content/entries/knowledge/photography.md