◆ Rebuild

Part 13 · Electricity

Lithium Batteries

Lithium-ion cells store four to six times as much energy per kilogram as lead-acid, which is why phones, laptops and electric cars exist. How they work, what their electrodes and electrolyte are made of, why they need careful charging circuits, why they catch fire, where lithium comes from, and the honest path from assembling packs out of cells to making cells yourself.

Difficulty
●●●●●
Time
An afternoon to build a small pack from tested cells; months to make the first workshop cell; a whole industry for cells as good as factory ones
Steps from zero
25 prerequisites →

You need first

The Rechargeable BatteryElectrolysis

This unlocks

SmartphonesElectric Vehicles
The full path from nothing — 25 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Lime
  14. Salt
  15. Fermentation
  16. Lye and Potash
  17. Glass
  18. Bellows
  19. Saltpeter
  20. Copper Smelting
  21. Lead
  22. Sulfuric Acid
  23. The Battery
  24. The Rechargeable Battery
  25. Electrolysis
  26. Lithium Batteries

Do them roughly in this order. See it on the tech tree →

Why it matters

A The Rechargeable Battery is cheap, tough and easy to make, and for a long time it is the right battery for a rebuilding society wherever weight does not matter. But it holds only about 30–40 watt-hours per kilogram: enough to drive a small car 100 km weighs nearly a tonne.

A lithium-ion cell holds 150–270 Wh/kg, four to six times as much. It loses only 1–3% of its charge a month, returns 95% of the energy put in, and lasts 1,000 to over 5,000 cycles. That made the mobile phone, the laptop and the practical electric car possible, and lets solar and wind power be stored in a box in a shed (Storing Energy).

The price: lithium cells are delicate and dangerous. Overcharge one by a tenth of a volt and it is damaged; abuse it badly and it bursts into a fire that is hard to put out. Every pack needs a protection circuit, and making cells needs bone-dry rooms, very pure chemicals and a petrochemical industry. This chapter starts with what a workshop can really do (test cells, build and protect packs), then shows where lithium comes from and how cells are made.

How it works

Lithium ions rocking between two hosts

Lithium is the lightest metal and the most eager to give away its electron, so a lithium cell gives 3.2–3.7 volts — nearly twice a lead-acid cell — from much lighter materials. Lithium metal is unsafe in a rechargeable cell: it plates back as needles (dendrites) that pierce the separator. So in a lithium-ion cell both electrodes are host materials, crystals with gaps where lithium ions can sit:

  • The negative electrode (anode) is usually graphite: sheets of carbon atoms stacked like pages, with lithium slipping between the pages. Six carbon atoms hold one lithium (LiC₆).
  • The positive electrode (cathode) is a metal compound holding lithium in its crystal: lithium cobalt oxide, lithium nickel-manganese-cobalt oxide (NMC), or lithium iron phosphate (LFP).

Charging pulls lithium ions out of the cathode, through the liquid, and in between the graphite sheets, while the charger pushes electrons round the outside wire. Discharging lets them flow back, and the electrons go round through your lamp or motor. Nothing dissolves or deposits; the lithium just rocks back and forth, which is why the cells last so long.

Lamp or motor electrons (discharge)electrons (discharge) discharge charge = lithium ion Copper foil8–10 µm, thenegative collector Anode: graphitelithium slips betweenthe carbon sheets Separatorporous plastic film,12–25 µm thick Cathode: LFP or NMCmetal phosphate or oxidegrains holding lithium Aluminiumfoil 12–20 µm,positive collector Electrolyte (blue): a lithium salt dissolved in dry organic carbonates, soaking everything between the foils –+
Fig. 1 A lithium-ion cell in cross-section. Lithium ions shuttle through the electrolyte and separator between graphite on copper foil and a metal oxide or phosphate on aluminium foil; electrons travel the same way through the outside circuit.

The other parts

  • Electrolyte. Water breaks down above about 1.5 V, so a 4 V cell cannot use it. Instead a lithium salt, usually lithium hexafluorophosphate (LiPF₆), is dissolved in dry organic liquids called carbonates. It is flammable, and a trace of water turns the salt into hydrofluoric acid.
  • Separator. Porous polyethylene or polypropylene film, 12–25 micrometres thick, that lets ions through but keeps the electrodes apart. At about 130 °C it softens and closes its pores: a fuse that works once.
  • Current collectors. The anode is coated on copper foil 8–10 µm thick, the cathode on aluminium foil 12–20 µm thick. They cannot be swapped: aluminium crumbles at the anode's voltage, copper dissolves at the cathode's.
  • The SEI. On the first charge, a little electrolyte breaks down on the graphite into a thin skin (the solid electrolyte interphase) that lets lithium through but stops further breakdown. Growing it slowly and evenly is the last step of manufacture and the secret of long life.

The chemistries

Cathode Volts (nominal / full) Cell Wh/kg Full cycles Made from Notes
Lithium cobalt oxide (LCO) 3.7 / 4.2 180–240 500–1,000 Cobalt Phones and laptops; burns fiercely
Nickel-manganese-cobalt (NMC) and nickel-cobalt-aluminium (NCA) 3.6–3.7 / 4.2 200–270 1,000–2,000 Nickel, some cobalt, manganese Most electric cars; best for weight
Lithium iron phosphate (LFP) 3.2 / 3.65 120–180 3,000–6,000 Iron and phosphate Safest, longest-lived; heavier for the same energy

For a rebuilt society, LFP is the chemistry to aim for. It needs no cobalt or nickel, only iron (Iron (the Bloomery)), phosphate (from rock phosphate, see Chemical Fertilisers) and lithium. It does not release oxygen when overheated, so it is far harder to set on fire, and it lasts several times longer.

What you need

To do You need See
Test cells Voltmeter reading to 0.01 V, ammeter, 4 Ω load resistor rated 10 W, clock Measuring Electricity
Charge cells Supply holding a set voltage within ±0.02 V, with current limit Rectifiers: Turning AC into DC, The Transformer
Build packs Nickel strip, spot welder, insulating card, fuses, thick copper cable Wiring and Electrical Safety
Protect packs Battery management system below, Semiconductors and the Transistor
Make cells Lithium carbonate, carbon, iron phosphate, foils, separator, electrolyte, argon dry box below, Liquid Air, Nitrogen and the Noble Gases

Where to find it

  • Spodumene, the main lithium ore, grows in pegmatites — very coarse granite veins with crystals fist-sized to metres long, among quartz, feldspar, mica and coloured tourmaline. Look for long, flat, grooved laths, greyish-white, pale green or lilac, as hard as quartz and heavier than feldspar. Good ore carries 1–2% lithium oxide.
  • Lepidolite, a pink-to-lilac lithium mica in the same veins: poorer, but easy to spot.
  • Salt-flat brine, the world's cheapest lithium, lies under dry salt flats (salars) in closed desert basins in volcanic highlands — the Andes of Chile, Argentina and Bolivia, Tibet, Nevada — and carries 0.02–0.2% lithium.
  • The test. Moisten crushed ore or dried brine with Hydrochloric Acid and hold it in a clean flame on a wire loop: lithium colours the flame crimson. Sodium's yellow often swamps it; a The Spectroscope shows lithium's red line at 671 nm clearly.

Seawater holds only 0.17 grams of lithium per tonne: far too little to work.

Method 1: Testing cells and building a pack

This is the most useful lithium work a small workshop can do, and how most packs in the world are made: cells joined by hand or machine. The same steps apply to home-made cells from Method 3.

The lithium-ion cell

A lithium-ion cell is one sealed unit: two long coated foils with separator film between them, wound into a roll or stacked in layers, soaked in electrolyte and closed in a can or pouch. Three shapes are common:

Form Size Typical content Notes
Cylindrical 18650 18 mm across, 65 mm long, 45–48 g 2.5–3.5 Ah at 3.6 V (9–12 Wh) Steel can; the commonest cell in laptops, tools and early cars
Prismatic Flat aluminium box, palm to brick size LFP: 100–300 Ah at 3.2 V; a 280 Ah cell weighs about 5.4 kg Solar storage, buses
Pouch Flat foil bag 0.5–60 Ah Phones; must be clamped flat
An 18650 cell, cut open +– 65 mm 18 mm Positive capwith safety vent Insulating disc Jelly rollanode foil, separator,cathode foil, separator,wound tight together Steel canis the negativeterminal A 4-cell pack in series (4S), seen from above +–+– Battery management system checks every cell, bleeds the fullest, and opens its switch if any cell is too full, too empty, too hot or overloaded Solid strips join cell tops; the dashed strip joins cell bottoms. Blue: sense wires to every junction. Thick: main current. Nickel strip, spot-welded (x) Temperaturesensor Fuse cut-off switch P–P+ output to charger and load
Fig. 2 Inside an 18650 cell, and a small four-cell pack with its battery management system. Cells are joined by spot-welded nickel strip; a sense wire runs to every junction between cells.

How to tell a good cell from a bad one:

  1. Look. Reject cells that are dented, rusty, leaking, or with torn wrap (a cylindrical cell's whole can is its negative terminal). Reject any pouch that has puffed up.
  2. Resting voltage. A healthy NMC cell rests between 3.0 and 4.2 V. One that has sat below 2.0 V for weeks may have grown copper threads inside; do not recharge it.
  3. Charge it (below). A cell that grows warm while charging at half its rated current is bad.
  4. Self-discharge. Rest it 14 days. A good cell loses under 0.05 V; one that loses more is leaking inside and may one day fail hot.
  5. Capacity. Discharge through a known resistor to 3.0 V and time it: amp-hours = current × hours. A 2 Ah cell through 4 Ω (about 0.9 A) should last over 2 hours. Below 80% of its rating, it is worn.
  6. Internal resistance. Voltage drop when the 4 Ω load goes on, divided by the current. Good 18650s: 20–60 milliohms. Above 120 mΩ, the cell sags and heats under load.

Group cells of the same type, age and capacity. A pack is only as good as its weakest cell.

The battery pack

A battery pack is cells joined in series for voltage and in parallel for capacity, with a fuse, a protection circuit and a case. Packs are named like 13S4P: 13 groups in series, each group 4 cells in parallel.

Count series cells from the nominal voltage: 3.6 V per NMC cell, 3.2 V per LFP cell. So 36 V is 10S NMC (42 V when full); 48 V is 13S NMC or 16S LFP. Four LFP cells in series (12.8 V, 14.6 V full) replace a 12 V lead-acid battery.

Step by step for a small 10S2P (36 V, about 6 Ah, 216 Wh) e-bike pack from 20 matched 18650 cells:

  1. Lay out the cells in a frame of plywood drilled with 18.5 mm holes, 1–2 mm apart for air.
  2. Join each parallel pair at both ends with nickel strip 0.15–0.2 mm thick and 8 mm wide (about 5–8 A per strip), then join the pairs in series, positive of one group to negative of the next.
  3. Weld, do not solder. More than two or three seconds of soldering iron cooks a cell's seal and separator. A spot welder presses two copper electrodes on the strip and passes 1,000–2,000 A for 10–50 milliseconds, from a capacitor bank or a large lead-acid battery switched by a heavy contactor. A good weld tears a hole in the strip when pulled off; practise on a dead cell.
  4. Sense wires to every junction between series groups, plus both ends (11 wires for 10S), for the protection circuit.
  5. Insulate every positive end with a ring of fish paper or card, and wrap the block.
  6. Fuse the positive lead, as close to the pack as possible. Better packs also join each cell through a short length of fine fuse wire, so one shorted cell cannot drain its neighbours.
  7. Fit the BMS (below) and a closed case of plywood or sheet metal.

The battery management system

A battery management system (BMS) keeps every cell inside its safe limits. A lead-acid battery forgives overcharging; a lithium cell does not. Cells in series drift apart over many cycles, so charging a 10S string to 42 V might push one cell to 4.4 V (damaged, a fire risk) while another sits at 4.0 V. A BMS does four jobs:

  1. Watches every cell. Above the upper limit (4.20 V for NMC, 3.65 V for LFP) it stops charging; below the lower limit (about 3.0 V NMC, 2.5 V LFP) it stops the load.
  2. Balances. Near full charge it bleeds the fullest cells through resistors so the rest catch up: 40 Ω across a 4.2 V cell bleeds about 100 mA.
  3. Limits current and heat. It cuts off on a short, on overload, above about 55 °C, and if charging below 0 °C.
  4. Switches, with power transistors in factory boards, or a heavy relay or contactor (The Electromagnet) in a workshop one.

A workshop BMS uses parts from Semiconductors and the Transistor. For each cell, a small transistor circuit compares the cell's voltage with a Zener reference diode; above 4.15 V it switches on that cell's bleed resistor. A second comparator per cell, set at the high and low limits, opens a contact in a chain wired in series with the coils of the main charge and load relays, so any one cell out of limits drops the relay. Many parts, one channel per series cell, but each part is simple.

Charging

Lithium cells are charged in two stages, constant current, then constant voltage (CC/CV):

  1. Constant current, usually half the capacity per hour (1 A for a 2 Ah cell), until the cell reaches 4.20 V (LFP: 3.65 V). This puts in about 80%.
  2. Constant voltage: hold exactly that voltage and let the current fall by itself. When it has dropped to a twentieth of the starting current, the cell is full.
  3. Switch off. Never trickle-charge or "float" a lithium cell at full voltage for days.

The upper voltage must be held within about ±0.05 V per cell, so the resistor charger of The Rechargeable Battery will not do. You need a regulated supply — transformer, rectifier, smoothing capacitor and a transistor regulator steered by a reference diode (Rectifiers: Turning AC into DC, Resistors, Capacitors and Coils) — checked against a voltmeter you trust.

For long life: charge only between 0 and 45 °C (below freezing, lithium plates out as metal); store at 40–60% charge, cool; and if you can spare the capacity, charge only to 4.1 V and stop at 3.3 V, which roughly doubles the cell's life.

Method 2: Getting lithium out of rock and brine

From brineFrom spodumene rock Brine wellunder a salt flat Evaporation pondssun and wind Add slaked limeMg drops out 0.02–0.2% lithium 12–18 months; salt andpotash crystallise out settle, draw offthe clear liquid Crush, sortpick pale crystals Roast1,050–1,100 °C Acid bakeacid, 250 °C Leach, cleanwater, lime, soda 1–2% lithium oxide;sort to about 6% crystal swells bya third, goes chalky lithium becomeslithium sulfate sand stays behind;Ca, Mg, Fe, Al out Heat to 80–95 °C,stir in soda ash Lithium carbonate Lithium carbonate dissolves less in hot water than in cold, so it falls out while sodium salts stay dissolved.
Fig. 3 Two routes to lithium carbonate. Brine is concentrated by the sun in shallow ponds; spodumene is roasted, baked with sulfuric acid and leached. Both end by adding soda ash to hot lithium solution, which drops lithium carbonate as a white powder.

Both routes are leaching chemistry of the kind in Leaching, Solvent Extraction and Electrowinning, and both end with lithium carbonate, the white powder from which every other lithium chemical is made. One unusual fact makes it work: lithium carbonate is less soluble in hot water than in cold (about 1.5 g per 100 mL at 0 °C, only 0.7 g at 100 °C). Add Soda Ash and Baking Soda to a hot, strong lithium solution and lithium carbonate falls out, while sodium and potassium salts stay dissolved.

From brine

  1. Evaporate in a chain of clay-lined ponds 30–50 cm deep. Common salt crystallises first, then potassium salts (fertiliser, Chemical Fertilisers). After 12–18 months the brine is a thick yellow liquid with about 6% lithium.
  2. Remove magnesium by stirring in slaked lime (Lime); it settles as white mud. Draw off the clear liquid.
  3. Precipitate. Heat to 80–95 °C and stir in strong soda-ash solution. Filter, wash with hot water and dry the white powder. For battery purity (above 99.5%), redissolve it in cold water with carbon dioxide bubbled through, filter, and boil to drop it out again.

From spodumene

  1. Crush and pick to 1–3 cm, sorting the pale spodumene from quartz and feldspar.
  2. Roast at 1,050–1,100 °C (bright orange to yellow, see The Kiln) for about an hour. The crystal swells by nearly a third and goes chalky. Raw spodumene resists acid; roasted, it does not.
  3. Acid bake. Grind to flour, mix with concentrated Sulfuric Acid (1 part to 3–4 parts ore by weight) and bake at about 250 °C for an hour. The lithium becomes lithium sulfate.
  4. Leach in water; lithium sulfate dissolves and the rest stays as sand. Add lime and soda ash to drop out calcium, magnesium, iron and aluminium. Filter.
  5. Precipitate lithium carbonate with hot soda ash, as for brine.

Expect to mine 30–40 tonnes of ordinary ore (1–2% lithium oxide), sort it down to 7–8 tonnes of rich spodumene, and get one tonne of lithium carbonate from that. In round terms, about 0.6 kg of lithium carbonate makes 1 kWh of LFP cells — so a tonne is enough for the batteries of 20–30 small electric cars, or for the night-time power stores of a dozen villages.

Lithium metal, for non-rechargeable cells, is made by Electrolysis of molten lithium and potassium chlorides at about 420 °C under dry argon.

Method 3: Making cells (the laboratory route)

Be clear about what this means. A skilled chemist in a rebuilding workshop can make small pouch cells that work, holding tens of milliamp-hours; reaching factory quality is the work of a whole industry. Learn on lead-acid and nickel-iron cells first. Attempt lithium cells once you have a chemical industry, Liquid Air, Nitrogen and the Noble Gases for argon and nitrogen, and a The Vacuum Pump.

The materials

  • Cathode: lithium iron phosphate. Mix lithium carbonate, iron(II) phosphate or iron oxalate (from iron and oxalic acid), and ammonium phosphate (from phosphoric acid and Ammonia) in exact proportions with about 10% sugar. Grind them together for hours in a ball mill. Heat to 650–750 °C for 8–12 hours in nitrogen or argon; the iron must not meet oxygen. (A covered steel box packed in charcoal powder, as in case hardening, see Steel, may serve when bottled gas is lacking.) The sugar chars to a film of carbon round every grain that carries the electrons. Good LFP is grey-black and gives about 150 mAh per gram.
  • Anode: graphite or hard carbon. Purified, finely milled flake graphite; or, easier, hard carbon — sugar, coconut shell or wood charred at 1,000–1,300 °C without air (Charcoal), giving 250–300 mAh/g. Early commercial cells used disordered carbons of this kind.
  • Binder to glue powder to foil: PVDF in the solvent NMP in industry; water-based cellulose or seaweed binders (carboxymethyl cellulose, alginate) work for graphite and LFP.
  • Foils: copper and aluminium rolled to 10–20 µm (Sheet Metal and Rolling, Aluminium).
  • Separator: porous polyethylene (Petrochemicals and Modern Plastics); glass-fibre paper 0.2 mm thick (Glass Fibre and Glass Wool) works in test cells.
  • Electrolyte — the hardest part. LiPF₆ needs anhydrous hydrofluoric acid, a job for a specialised chemical works; the carbonate solvents are petrochemicals (Petroleum and Refining). One trap: pure propylene carbonate, the easiest solvent, splits graphite apart; use hard carbon with it.

Making a pouch cell

  1. Slurry: 90 parts active powder, 5 parts carbon black (lamp soot works), 5 parts binder, and solvent to make a paste like thick cream.
  2. Coat the foil with a blade set 100–150 µm above it. Dry at 80–120 °C, then under vacuum for 12 hours.
  3. Press between polished steel rollers to about two-thirds the thickness. A good electrode is smooth, dark, and does not flake when bent round a pencil.
  4. Cut a cathode 4 × 4 cm and an anode 4.2 × 4.2 cm (always slightly bigger, so no lithium plates at its edge), each with a bare foil tab.
  5. Assemble in the dry box — a sealed box with glove ports, filled with argon and dried with phosphorus pentoxide (Phosphorus). Water must stay below about 20 parts per million; one breath ruins a cell. Stack anode, separator, cathode in a bag of plastic-laminated aluminium foil, add a few drops of electrolyte, heat-seal it with the tabs out.
  6. Form it: a very slow first charge over about 20 hours while the SEI grows.
  7. Test it as in Method 1. Expect 30–40 mAh. If it keeps most of that after 50 cycles, you have succeeded.

In a factory, the same steps run on rolls of foil a metre wide and kilometres long: coating lines 50–100 m long with drying ovens, rollers holding thickness to ±2 µm, winding into "jelly rolls", laser-welded lids, filling under vacuum, then formation and ageing for one to three weeks on racks of thousands of chargers, all in dry rooms with a dew point of −40 °C or below. That mix of chemistry, precision machinery and patience is why only a few dozen places on Earth make good cells.

How to tell it worked

  • A pack charges to its full voltage with every cell within 0.02 V of the others, and stays there for a week.
  • Under its normal load, no cell and no strip gets more than warm.
  • The BMS really cuts off: test it by feeding one sense input from an adjustable supply and raising it past the upper limit, then lowering it past the lower one. The relay must drop both times.
  • A home-made cell gives a sloping voltage (NMC) or a long flat plateau near 3.3 V (LFP) on discharge, and returns most of the charge put in.

Note Troubleshooting. One cell group always ends full first or empty first → it has less capacity or more self-discharge. Swap in a better-matched cell, or let the balancer run longer. Pack voltage sags badly under load → cells with high internal resistance, or a weak weld or thin strip. Feel for warm spots after a hard run. Home-made cell gives almost nothing → water in the dry box, oxidised LFP (rusty brown instead of grey-black), graphite split by propylene carbonate, or the separator leaking. Fix the dryness first; it is almost always that. Pouch swells → water or overcharge made gas. Stop using it.

Dangers

Danger Thermal runaway. A shorted, punctured, crushed, overcharged or badly overheated lithium cell can heat itself, faster and faster, past 600 °C in seconds. It vents a jet of flammable, poisonous gas (carbon monoxide and hydrogen fluoride) that often catches fire, and the heat sets off its neighbours one after another. It cannot be smothered, because the cathode supplies its own oxygen. Charge packs on stone, brick or a metal tray, away from anything that burns, never unattended overnight. If a pack smokes or hisses, get everyone out; only if it is safe, push it outdoors onto bare ground. Large amounts of water cool the cells and stop the spread; a small extinguisher does not.

Danger Hydrofluoric acid. The electrolyte salt and the smoke from a burning cell form hydrofluoric acid with any moisture. It passes through skin without much pain at first and attacks bone and the heart's rhythm. Handle electrolyte only with gloves and goggles in a dry box, with calcium gluconate gel within reach. Treat a skin splash by washing under running water for about 5 minutes, then rubbing in calcium gluconate gel at once and for at least 15 minutes; wash eyes for 15 minutes; then get medical help (first aid in full in Fluorspar and Fluorine Compounds). Chalk paste is useless.

  • Short circuits. One 18650 can push 30–60 A into a short, enough to weld a ring to the terminal and burn to the bone. Take off rings; use insulated tools; cover pack terminals.
  • Lithium metal catches fire with water. Store it under mineral oil.
  • Dust and solvents. Cobalt and nickel powders cause cancer and asthma; the solvent NMP harms unborn babies. Work wet or in a hood.
  • Damaged cells — crushed, swollen, or left below 2 V — are fires waiting to start. Discharge them slowly through a resistor outdoors and store them in a metal box of sand.

What this unlocks

Light, powerful packs make the electric bicycle and car practical, power cordless tools and robots, and store solar and wind power (Solar Cells, Wind Turbines, Storing Energy). Together with Microprocessors and Personal Computers and Flat Screens: LCD and LED Displays they make the smartphone possible. If lithium is scarce, sodium-ion cells — the same idea with sodium from common salt and hard-carbon anodes, about two-thirds the energy — are a sensible second path.

How it was first done

Johan August Arfwedson discovered lithium in Sweden in 1817; Robert Bunsen and Augustus Matthiessen made the metal in quantity in 1855 by electrolysis. Non-rechargeable lithium cells reached the market in the 1970s. In 1976 M. Stanley Whittingham, working for Exxon, showed a rechargeable cell with a titanium disulfide cathode and a lithium metal anode, but it was prone to fire. In 1980 John Goodenough and his team at Oxford found that lithium cobalt oxide gave about 4 V. In 1985 Akira Yoshino at Asahi Kasei in Japan paired it with a carbon anode instead of lithium metal: the first true lithium-ion cell. Sony began selling them in 1991, for video cameras. Goodenough's group described lithium iron phosphate in 1997. Goodenough, Whittingham and Yoshino shared the Nobel Prize in Chemistry in 2019.

Source: content/entries/electricity/lithium-batteries.md