Part 8 · Chemistry
Rubber
Cut the bark of a rubber tree and a white milk runs out. Set it with a little vinegar, dry it, knead in sulfur and bake it, and you have a material that stretches, springs back and keeps out water — for seals, hoses, tyres and electrical insulation.
- Difficulty
- ●●●●●
- Time
- Trees take 6–7 years to reach tapping size; a morning to tap, a day to set, one to two weeks to dry; an afternoon to compound and 2–3 hours to cure
- Steps from zero
- 1 prerequisite →
You need first
SulfurThe full path from nothing — 1 step before this one
- Sulfur
- Rubber
Do them roughly in this order. See it on the tech tree →
Why it matters
Almost every machine in the second half of this book needs something soft that seals. A pump needs a leather or rubber cup; a steam engine needs gaskets; a canning jar needs a ring; a bicycle needs a tyre; an electric wire needs a skin that keeps the current in and the rain out. Leather, cork, oiled hemp and wax will do for a while, but nothing does all of these jobs as well as rubber: it stretches to several times its length and snaps back, does not let water or air through, does not conduct electricity, and lasts for years.
Raw rubber straight from the tree is a disappointment: it turns sticky in summer sun and stiff and brittle in frost. The trick that turned it into one of the great materials of industry is vulcanisation — baking it with a few percent of Sulfur. With much more sulfur it becomes hard rubber (ebonite), a black, hornlike solid you can saw, drill and polish, and the best electrical insulator of the nineteenth century.
Rubber leads to waterproof cloth and boots (Making Clothes, Footwear), tyres for the The Bicycle and The Motor Vehicle, seals for Canning and Bottling, pumps and the The Steam Engine, hoses for Welding and fire-fighting, insulation for Copper Wire and the The Telegraph, and balloons (Balloons).
How it works
Many plants make a milky sap called latex in a network of tiny tubes in their bark or leaves. When the plant is wounded, latex runs out and seals the wound. In a few plants, a third or more of that latex is tiny droplets of rubber floating in water, each wrapped in a thin skin of protein that keeps the droplets apart.
- Coagulation. Make the latex slightly sour (add vinegar or another acid) and the protein skins stop repelling each other. The droplets clump into a soft, white, spongy curd — just as milk curdles into cheese. Squeeze out the water and dry it and you have raw rubber.
- Why raw rubber is weak. Rubber is made of enormously long, tangled, chain-like molecules. Pull it and the chains straighten; let go and they curl back up — that is its stretch. But the chains are not tied to each other, so when warm they slide past one another (sticky, it creeps and flows), and when cold they stiffen.
- Vulcanisation. Heated to about 140 °C with sulfur, the sulfur forms short bridges between neighbouring chains, tying them into one huge net. Now the chains can still uncurl and recoil, but they cannot slide. The rubber stays springy from well below freezing to above the boiling point of water, and no longer dissolves in oils and turpentine — it only swells.
- More sulfur, harder rubber. A few parts of sulfur to 100 of rubber gives soft rubber. A third to a half as much sulfur as rubber ties the chains so tightly that nothing can move: hard rubber.
- Mastication. Raw rubber is too tough and springy to mix powders into. Working it hard between rollers or kneading it on a warm slab tears some of the long chains, and it becomes soft and doughy, like putty. Then sulfur and fillers can be kneaded in.
What you need
| Item | Amount | Notes |
|---|---|---|
| Rubber trees or latex plants | 10–50 trees for a small workshop | See below. A good tree gives 2–4 kg of dry rubber a year. |
| Tapping knife | 1 | A small, sharp hooked blade or a gouge made from a scrap of Steel; see Axes, Chisels, Knives and Planes |
| Spouts and cups | 1 per tree | A strip of tin, bamboo or a leaf as a spout; a coconut shell, gourd or small pot as a cup |
| Settling pans | Several | Shallow trays of wood, clay or tin about 40 × 30 × 10 cm |
| Vinegar | About 1 cup (250 ml) per 4 litres of diluted latex | Ordinary vinegar from Fermentation. Alum also works. |
| Sulfur, finely powdered | 2–10 parts per 100 of rubber (soft); 30–50 (hard rubber) | See Sulfur. Sieve through fine cloth. |
| Fillers (optional) | Up to equal weight with the rubber | Fine chalk (cheap, stiffer); soot or lampblack (tough, wear-resistant — for tyres and soles) |
| Slaked lime or wood ash (optional) | 2–5 parts per 100 | Speeds the cure. See Lime. |
| Rolling pin and a smooth stone slab or board | 1 | Or two hardwood rollers on a frame |
| Moulds, an iron box, a sand bath | — | For curing. See below. |
Where to find it
Rubber plants are mostly tropical, but there are temperate and desert ones. Test any plant with milky sap: let a few drops dry on your fingertip, then rub. If it rolls into a little elastic ball that bounces and stretches, there is rubber in it. If it dries into a brittle or gummy film, there is not.
- Pará rubber tree (Hevea brasiliensis). The best rubber there is. A tall, straight tree with smooth grey bark and leaves in threes (each leaf split into three long leaflets), wild in the Amazon basin and planted across the wet tropics of Asia and Africa. Fruits are three-lobed capsules that burst with a crack and scatter mottled seeds. Old plantations persist for generations and seed themselves.
- Panama rubber tree (Castilla elastica) of Mexico and Central America; India rubber fig (Ficus elastica, the big glossy-leaved "rubber plant") of north-east India and South-East Asia; Landolphia vines of tropical Africa; Ceará rubber (Manihot glaziovii), a relative of cassava. All give useful but stickier or weaker rubber.
- Guayule (Parthenium argentatum). A small silvery-grey shrub, knee-high, of the Chihuahuan desert in northern Mexico and south-west Texas. It has no running latex: the rubber sits inside the cells of bark and roots, 10–20% of the dry weight in older plants.
- Rubber dandelion (Taraxacum kok-saghyz). A small dandelion with blue-grey leaves from the mountains of Kazakhstan, grown as a crop in the Soviet Union in the 1930s–40s. The roots hold roughly 5–10% rubber; snap one and the white sap pulls into threads. The common dandelion has very little — not worth processing.
- Not rubber. Spurges (Euphorbia), milkweeds and poppies have milky sap, but mostly resin and very little rubber; spurge sap blisters skin and can blind (see Dangers). Gutta-percha and balata trees of South-East Asia and South America give a related gum that softens in hot water and sets hard but is not elastic — excellent for insulating underwater cables and for moulding (Early Plastics).
Step by step
1. Tap the tree
- Choose trees with a trunk at least 50 cm round (about two hand-spans across) at 1 m height — six or seven years old for Hevea.
- Mark the cut. Starting about 1.2–1.5 m above the ground, mark a line sloping downward from upper left to lower right at about 25–30° and running halfway round the trunk. The latex tubes spiral slightly up the trunk the other way, so this slope cuts across the most of them.
- Fix a spout at the low end — a strip of tin or bamboo pushed into the bark — and hang a cup under it.
- Tap at dawn. Latex flows best in the cool early morning, when the tree is full of water. With the knife, shave a sliver of bark 1–1.5 mm thick off the lower edge of the cut. Go deep enough that latex beads along the whole cut, but never through to the cambium — the thin, green, wet layer just over the wood. Leave about 1 mm of bark there. Cut into the cambium and the tree grows lumps and you lose that panel.
- Collect after 2–3 hours, when the dripping stops. A good tree gives 100–250 ml (half a cup to a cup) per tapping, about a third of it rubber. Peel off the thin strip of rubber that dries in the cut ("scrap") and keep it — it is lower-grade rubber.
- Rest the tree. Tap every second or third day. Each tapping uses only a thin shaving, so a panel lasts years. When you reach the ground, move to the other half of the trunk; the first side heals and can be cut again.
Tip Keeping latex liquid. Latex starts to set by itself within a few hours. If you must carry it far, stir in a spoonful (10–15 ml) of strong ammonia water per litre (Ammonia) and keep it covered and cool. Without ammonia, set it the same day.
Other plants. For guayule and rubber dandelion, pull the whole plant or roots, dry them for a week, then crush them in plenty of water with a heavy pestle or between millstones (The Watermill). The rubber clumps into soft, grey, worm-like threads that float; the woody bits sink. Skim the "worms", wash, press and dry. Guayule rubber contains sticky resin; soaking it in acetone for a day removes most of it.
2. Set the rubber
- Strain the latex through a fine cloth into a settling pan, to catch bark and insects.
- Dilute with about an equal volume of clean water. Thinner latex sets into a more even, easily dried sheet.
- Add vinegar slowly while stirring, about a cup (250 ml) per 4 litres of diluted latex. Skim off the froth. Too much acid gives a hard, uneven curd; too little sets slowly or not at all.
- Leave covered overnight. In the morning you have a white, wobbly slab floating in clear, yellowish water. Cloudy, milky water means it did not all set — add a little more vinegar next time.
3. Press, dry and smoke
- Press the slab by hand on a board, then roll it with a wooden rolling pin or between two wooden rollers to a sheet 3–4 mm thick, washing it with clean water as you go. Water should squeeze out clear.
- Drip-dry in the shade for a day.
- Dry for one to two weeks hanging on poles in a shaded, airy shed, or faster (4–7 days) in a smokehouse at about 40–60 °C — warm like a sunny wall, not hot to the hand. Smoke stops mould. The Amazonian way is the same idea: latex is ladled onto a paddle and turned in the thick smoke of palm nuts, layer upon layer, until it builds into a big ball.
- Done when the sheet is evenly amber to brown and see-through when held to the light, with no white patches (white = still wet inside). Store in a cool dark place.
At this stage you can already use it: dissolved in turpentine or naphtha (it takes days of soaking to swell and dissolve), it makes rubber cement, a glue and a waterproof coating for cloth. But for anything that must stay springy, vulcanise it.
4. Masticate and mix
- Warm the slab or board to about 60–70 °C — just too hot to keep your hand on.
- Knead. Fold, roll and press a lump of dry rubber again and again, or pass it many times between two hardwood rollers turning at slightly different speeds. After 10–20 minutes it stops springing back and turns soft and doughy.
- Sprinkle in the powders a little at a time, folding them in until the colour is perfectly even, with no streaks. A starting recipe, by weight:
| For | Rubber | Sulfur | Lime | Filler |
|---|---|---|---|---|
| Soft rubber (seals, tubing, rings) | 100 | 5–8 | 3 | 20–50 chalk |
| Tough rubber (soles, tyres) | 100 | 5–8 | 3 | 30–50 soot or lampblack |
| Hard rubber (ebonite) | 100 | 35–50 | — | 0–20 chalk |
5. Shape
- Sheet: roll to thickness between two boards with strips of the right thickness as guides.
- Seals and rings: press into a two-part mould of metal, hard-fired clay or hardwood, slightly overfilled so excess squeezes out.
- Tubing and hose: wrap rubbered cloth, or a rolled sheet with overlapping seam, round a smooth greased rod (mandrel); bind tightly with a spiral of wet cloth tape that squeezes it as it cures; pull the rod out afterwards.
- Waterproof cloth: spread rubber cement thinly on cloth, let the solvent evaporate, and cure.
6. Cure (vulcanise)
- Dust the pieces with chalk or fine ash so they do not stick, and bury them in fine dry sand or chalk powder in an iron box or clay pot. Moulds are clamped and buried the same way.
- Set the box in a sand bath over a gentle fire, or in a bread oven as it cools.
- Judge the heat with sulfur. Put a pinch of sulfur on the sand right next to the box. Sulfur melts at about 115 °C into a thin, clear yellow liquid; above about 160 °C it turns dark red-brown and thick like treacle. Keep it melted and yellow-orange, never dark — that holds you near 130–150 °C.
- Time — for soft rubber 1–3 hours depending on thickness (add half an hour per extra 5 mm). Hard rubber needs 5–10 hours, raised slowly, as it shrinks and gives off foul gas.
- Cool slowly in the box before unpacking.
How to tell it worked
- Stretch test. Pull a strip of soft rubber to three times its length and let go: it should snap straight back with no permanent sag.
- Heat and cold. A strip left a day on a hot rock in the sun stays dry and not tacky; a strip left overnight on ice still bends without cracking. Uncured rubber fails both.
- Solvent test. A small piece soaked a day in turpentine swells but stays in one piece. Raw rubber goes to slime.
- Hard rubber is black-brown, rings when tapped, can be sawn, filed and polished like horn, and bends a little before snapping.
- Smell. Cured rubber smells faintly of sulfur; a strong rotten-egg smell means too much sulfur or too hot.
Note Troubleshooting. Latex won't set → too little acid, or it was diluted too much. Add vinegar a spoonful at a time. In cold weather, give it longer. Sheets mouldy or white inside → too thick or dried too slowly. Roll thinner, use the smokehouse. Rubber sticky after curing → undercured: too cool, too short, or too little sulfur. Cure again for longer. Rubber hard, cracks when bent → overcured: too hot or too long. Cut the time and watch the sulfur pinch. Bubbles and blisters in the cured piece → trapped water or air. Dry the sheets fully, knead more, press moulds harder, and warm up more slowly. Yellow bloom on the surface → excess sulfur coming out. Use less next time; it is harmless.
Dangers
Danger Rotten-egg gas. Heating rubber with sulfur, especially hard rubber, gives off hydrogen sulfide. At high levels it deadens your sense of smell within minutes — so the smell going away does not mean the gas has gone — then causes collapse and death. Cure only in the open air or a well-ventilated shed, never in a closed room, and never lean into an opened curing box. If the sulfur ever catches fire it makes choking sulfur dioxide too.
Warning Milky saps that burn. Spurge (Euphorbia) and some fig and milkweed saps blister skin and can blind if they reach the eyes. When testing unknown plants, keep sap off your face, wash hands afterwards, and rinse eyes with plenty of water at once if splashed.
- Latex allergy. Some people become allergic to rubber-tree latex proteins: itching and rash, sometimes swelling of the throat. Anyone who reacts should not handle latex.
- Fire. Rubber cement made with turpentine or naphtha is very flammable — mix it far from flames (Ether, Acetone and Solvents). Burning rubber gives thick, poisonous smoke.
- Hot sulfur sticks to skin and burns deeply; cool any burn in water for 20 minutes (Wound Care and Antiseptics).
- Do not use white lead or other lead compounds in rubber, though old makers did — they are poisons (Lead).
- Trees. Over-tapping or cutting into the cambium kills trees that took seven years to grow.
What this unlocks
- Seals and gaskets for pumps, Canning and Bottling jars, the The Steam Engine and engines, and the rubber rings and valves of the The Vacuum Pump.
- Insulated wire. Wrap Copper Wire in a strip of rubber with a cloth tape over it and cure. Sulfur attacks bare copper, so tin the wire first (Tin and Pewter) — this is why old rubber-covered wire is silvery inside. This made the The Telegraph, house wiring (Wiring and Electrical Safety) and the The Telephone practical.
- Tyres. First solid rubber bands on wheels; then air-filled tyres with cloth layers for the The Bicycle and The Motor Vehicle. Soot-filled rubber wears many times longer than plain.
- Hard rubber for battery boxes (The Rechargeable Battery), instrument parts, combs, pens and insulating panels (Early Plastics).
- Rubberised cloth for rainwear, tents, gas bags and hoses (Making Clothes, Raincoats, Oilskins, Umbrellas and Rubber Boots).
- Rubber thread, cut from thin cured sheet and wrapped in cotton, for the Elastic and Rubber Thread of clothing, rubber bands and support bandages.
How it was first done
The peoples of Mesoamerica were making rubber at least 3,600 years ago; the Olmec — the name means "rubber people" in Nahuatl — made solid rubber balls for their ritual ballgame, and later peoples made sandals and bands. Archaeologists think they mixed the latex of Castilla with the juice of a morning glory vine, which made it tougher and bouncier — a natural form of curing.
The French explorer Charles-Marie de La Condamine sent samples from the Amazon to Paris in the 1740s. In 1770 Joseph Priestley noted that it rubbed out pencil marks, hence the English name. Charles Macintosh patented waterproof cloth — rubber dissolved in coal-tar naphtha between two layers of fabric — in 1823, and Thomas Hancock invented his masticating machine around 1820. Both suffered from the same problem: the goods turned to glue in summer.
In 1839 Charles Goodyear, in Massachusetts, found by accident that rubber mixed with sulfur and heated stayed elastic in heat and cold; he patented it in 1844. Hancock, examining Goodyear's samples, worked out the process independently in England in 1843, and the name "vulcanisation" — after Vulcan, god of fire — was coined by his friend William Brockedon. In 1876 Henry Wickham carried Hevea seeds from Brazil to Kew Gardens in London, and from there plantations spread across South-East Asia. John Boyd Dunlop's air-filled bicycle tyre (1888) and the motor car turned rubber into one of the world's most important crops. The demand also brought terrible cruelty: in the Congo Free State and the Putumayo region of the Amazon, forced rubber collection around 1900 killed enormous numbers of people. Synthetic rubbers, made from coal, oil and alcohol, came in the 1930s and 1940s (Synthetic Rubber Works (Overview), Calcium Carbide and Acetylene, Petroleum and Refining).
Source: content/entries/chemistry/natural-rubber.md