◆ Rebuild

Part 13 · Electricity

Copper Wire

How to purify copper, pull it into long, even wire through a hardened steel draw plate, and cover it so it does not leak electricity. Every coil, magnet, motor, generator and telegraph line is made of this.

Difficulty
●●●●●
Time
A week to make a draw plate and bench; then a day per few hundred metres of wire
Steps from zero
14 prerequisites →

You need first

Copper SmeltingBlacksmithing

This unlocks

The ElectromagnetThe GeneratorThe TelegraphThermocouples and ThermoelectricityWiring and Electrical SafetyResistors, Capacitors and CoilsIron and Brass Wire
The full path from nothing — 14 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Copper Smelting
  13. Iron (the Bloomery)
  14. Blacksmithing
  15. Copper Wire

Do them roughly in this order. See it on the tech tree →

Why it matters

Electricity is useless if you cannot lead it where you want it. A wire is a road for electric current, and a coil — wire wound round and round — is how electricity is turned into magnetism and back again. Every The Electromagnet, The Electric Motor, The Generator, The Telegraph, The Telephone and Radio in this book is mostly wire, wound with care.

Wire also makes chain, Springs, sieves and pins, but for electrical work it has to be long (tens to hundreds of metres in one piece), even in thickness, pure, and insulated — covered so that current cannot jump from one turn to the next. This chapter covers all four.

How it works

Why copper

A metal carries electricity because some of its electrons are free to drift between atoms. How easily they drift varies a great deal between metals:

Metal How well it conducts (copper = 100) Notes
Silver 105 Best of all, but rare
Copper 100 Cheap, soft, easy to draw
Gold 70 Too rare
Brass 25–30 See Zinc and Brass
Iron and soft steel 15–17 Works for long outdoor lines if made thick
Lead 8 Poor

Copper is the best conductor you can make in quantity. It is soft enough to pull through a hole cold, it does not rust away, and it can be joined by twisting and soldering. Iron wire carries current about six times worse, so an iron wire needs about six times the cross-section to do the same job — fine for an outdoor line on poles, poor for a coil where space is tight.

Why purity matters

Small amounts of iron, arsenic, sulfur or antimony — all common in copper ores — make copper conduct much worse; some trade copper of the 1850s conducted only half as well as pure copper. In a tool that does not matter. In a coil, it wastes half your battery.

What drawing does

Drawing means pulling a rod through a hole slightly smaller than itself. The metal cannot tear because it is gripped evenly all round, so it flows: it gets thinner and longer. Each hole can only reduce the thickness by a little — about a tenth — so you pull it through a series of smaller and smaller holes.

Pulling also work-hardens copper: each pass makes it stiffer and more springy, until it would snap. Annealing — heating it to a dull red and cooling it — makes it soft again. Wire-making is a rhythm of draw, draw, draw, anneal.

What you need

Item Size or amount Where from
Copper 1 kg makes about 140 m of 1 mm wire, or about 570 m of 0.5 mm wire Copper Smelting
High-carbon steel bar for the draw plate about 20 × 4 × 1 cm Steel
Forge, anvil, hammers, tongs — Blacksmithing
Crucible and charcoal crucible for 1–2 kg of copper Pottery, Charcoal, Metal Casting
Draw tongs heavy pliers with ridged jaws, 30 cm handles forge them
Draw bench with windlass a heavy log or bench, 2 m long Basic Woodworking
Lubricant beeswax, tallow or soap Beekeeping, animal fat, Soap
Insulation silk or cotton thread, shellac or oil varnish, paper, wax see below
A file for pointing the wire Files and Saws

Where to find it

  • Copper comes from smelting ore — see Finding and Identifying Ores and Copper Smelting. Native copper (pure metal found as lumps and branching sheets in rock) occurs in some places, notably around Lake Superior; it is already very pure and ideal for wire.
  • Beeswax from wild or kept bees (Beekeeping). Tallow is rendered animal fat (beef or mutton fat melted and strained).
  • Silk comes from the cocoons of silk moths; cotton from the seed fluff of cotton plants; linen thread from flax (Spinning and Weaving Cloth).
  • Lac, the raw material of shellac, is the orange-brown resin crust that tiny lac insects leave on tree twigs in India, Thailand, Burma and southern China. Scrape it off, crush it, wash out the red dye, then melt and strain it. Elsewhere, use the oil varnish or wax described below.

Step 1: Purify the copper (fire refining)

Smelted copper is usually full of iron, sulfur and other metals. Fire refining removes most of them using air and then green wood.

  1. Melt the copper in a crucible in a charcoal forge or furnace with a strong blast (see Bellows). Copper melts at 1,085 °C — bright yellow-orange heat.
  2. Oxidise. Blow air across the surface of the melt for 15–30 minutes (rake back the charcoal, or direct a bellows nozzle at it). Iron, zinc, sulfur and lead react with the air faster than copper does. They form a crust of dross and slag. Skim it off with a dry iron or green-wood rake. Repeat until little new scum forms.
  3. Test. Dip the end of a cold iron rod in the melt and let a small blob freeze on it. Break the blob. If it breaks easily and the fracture is coarse and dark brick-red, the copper has taken up too much oxygen.
  4. Pole. Cover the melt with a layer of crushed charcoal, and push a stick of green, sappy wood (a pole as thick as your wrist) down into it. It will hiss and boil violently as the wood gives off gases that pull the oxygen back out of the copper. Keep stirring with fresh green sticks for 10–20 minutes.
  5. Test again. Now a test blob should be tough to break, and the broken face should be fine-grained, silky and salmon-pink. Stop then. If you go too far, the copper turns brittle again ("overpoled"); blow air across it for a few minutes and re-test.
  6. Cast into rods. Pour into a straight open groove cut in a block of soft stone, dried clay or sand (Metal Casting): about 1.5 cm wide, 1.5 cm deep, 25–30 cm long. Each rod weighs about 0.5 kg.

Tip If you can make electricity already, the purest copper of all comes from Electrolysis: impure copper slowly dissolves at one plate and pure copper builds up on the other. All modern electrical copper is refined this way.

Step 2: Forge the rod

  1. Hammer the bar round and thinner, cold, on the anvil — copper can be worked cold. Turn it a quarter turn between blows to keep it square, then knock off the corners to make it eight-sided, then round.
  2. Anneal whenever it starts to feel hard and springy under the hammer, or every 5–10 minutes of work: heat it to a dull red (500–600 °C, the first red you can see in a shaded place) and drop it in water. Quenching does not harden copper as it does steel; it leaves it soft, and the shock cracks off the black scale.
  3. Stop when the rod is 5–6 mm thick, even and round, with no cracks or folds. Folds or splits will break when drawn — cut them out.
  4. Point one end: file or hammer the last 4 cm into a long taper, so it pokes through each hole far enough for the tongs to grab.

Step 3: Make the draw plate

The draw plate is the one precise tool in this chapter. Take your time: a good plate lasts a lifetime.

FRONT FACE OF THE PLATE 5 mm each hole about one-tenth smaller across … on to 0.5 mm, about 24 holes SECTION THROUGH ONE HOLE (the step is drawn exaggerated) Back face wide funnel entry Front face hole at its working size Hardened steel plate about 1 cm thick Wire ingreased with wax or tallow Wire out thinner and longer Draw tongs pull steadily, no jerks
Fig. 1 The draw plate. Each hole is a funnel that narrows towards the front face. The wire goes in at the wide back, is squeezed thinner, and comes out the front.
  1. Forge the blank from high-carbon Steel: a flat bar about 20 cm long, 4 cm wide and 1 cm thick. Hammer it flat and true.

  2. Soften it. Heat it to red and bury it in dry wood ash to cool slowly overnight. Soft steel can be drilled and filed.

  3. Mark out a row of holes about 6–7 mm apart, centre to centre. You need about 24 holes to go from 5 mm down to 0.5 mm. Use two plates if one is too short: a coarse plate (5 mm → 1.5 mm) and a fine plate (1.5 mm → 0.3 mm).

  4. Drill each hole right through, smaller than its final size, with a bow drill or The Lathe-driven drill. Alternatively punch them while the plate is red-hot, using a round tapered punch, driven in from the back face.

  5. Taper each hole. Make a tapered reamer: a steel rod filed into a long, gentle cone with four sharp edges (square in section), hardened. Ream each hole from the back face only, so every hole is a funnel: wide at the back, narrowing to its working size at the front. The funnel should narrow over most of the plate's thickness — a gentle cone, not a sharp step.

  6. Size the holes. Each hole should be about one-tenth smaller across than the one before. A practical series in millimetres:

    5.0 · 4.5 · 4.1 · 3.7 · 3.3 · 3.0 · 2.7 · 2.4 · 2.2 · 2.0 · 1.8 · 1.6 · 1.45 · 1.3 · 1.2 · 1.05 · 0.95 · 0.85 · 0.77 · 0.7 · 0.63 · 0.57 · 0.51

    You will not hit these exactly. What matters is that each step is small and even. Check them by pushing a test wire: it should enter the next hole about halfway up its point, then stop.

  7. Polish the inside of each hole with a smooth taper of hard wood charged with fine sand and oil, then with fine charcoal dust or rouge (iron oxide) in oil. Rough holes scratch and tear the wire.

  8. Harden. Heat the whole plate evenly to cherry red (about 800 °C) and quench it in water or brine. Then temper: polish one face and warm the plate gently over coals until the bright face turns pale straw-yellow (about 220 °C), and cool it. This leaves it hard enough to keep its holes but not so brittle it cracks under the pull (hardening and tempering are explained fully in Forge Shops and Heat Treatment).

  9. Number the holes with a punch or file marks so you always go in order.

Note Holes wear larger with use. When one wears, you can close it slightly by softening the plate again and tapping around the hole on the front face with a round-ended punch, then re-reaming and re-hardening.

Step 4: Build the draw bench

Copper rod annealed and greased Draw plate back face towards the rod Stop stout pegs take the pull Draw tongs the pull squeezes the jaws pull Rope or chain Windlass 12 cm drum, 50 cm arms Bench heavy plank or log, about 2 m
Fig. 2 A simple draw bench. The plate rests against two stout pegs; the wire is gripped by draw tongs, and a windlass winds in the rope. The harder you pull, the tighter the tongs grip.
  1. Take a heavy plank or split log about 2 m long. Near one end, fix two strong pegs or an iron stop with a gap between them for the wire to pass. The draw plate rests flat against them, back face towards the incoming rod.
  2. At the other end, fit a windlass: a wooden drum 10–15 cm across on an axle, turned by two crossed handles about 50 cm long. A rope or chain runs from the drum to the draw tongs. A windlass with 50 cm handles and a 12 cm drum multiplies your pull about eight times (Simple Machines).
  3. Draw tongs have ridged jaws and handles that curve outward; a ring or a loop of rope goes round the handles and connects to the windlass rope, so the pull itself squeezes the jaws shut.

How much pull you need, roughly: drawing 4–5 mm copper takes a pull of about 100–200 kg — windlass work. At 3 mm it is about 50–70 kg (Iron and Brass Wire), and at 2 mm about 25–35 kg. Below 1.5 mm one person can pull it with hand tongs, and below 1 mm you can wind the wire onto a hand-cranked wooden drum 20–30 cm across, which also stores it neatly.

Step 5: Draw the wire

  1. Grease the rod: rub it with beeswax, tallow or soft soap, or draw it through a pad of greased leather before the plate (Lubricants and Greases). Dry drawing tears the wire and wears the plate.
  2. Feed the point through the first hole it fits, from the back face.
  3. Grip and pull smoothly and steadily, without jerking, until the whole length is through. Steady pulling gives even wire; jerks make thin spots.
  4. Repoint the end with a file if needed, and go to the next hole.
  5. Anneal every 3–4 holes, or sooner if the wire feels springy and fights you when you bend it. Coil the wire loosely, heat the coil to dull red, and quench in water. For thin wire (below 1.5 mm), anneal the coil inside a closed clay pot with a handful of charcoal dust, so that it does not burn away in the air; let the pot glow dull red for 10 minutes and tip the coil into water.
  6. Clean the black scale off after annealing by soaking the coil for an hour in vinegar with a spoonful of salt per cup (Vinegar and Pickling), then rinsing. Scale left on the wire scores the plate.
  7. Stop at the size you need. Give the last pass without annealing: slightly hard wire keeps its shape better in coils. Anneal it if it must be bent tightly.

Joining lengths. You will often need longer wire than one rod gives. Scrape both ends bright, overlap them by 3 cm, twist them tightly together round each other, and solder the joint (a tin–lead solder, see Soldering and Brazing) or at least wrap it tight and varnish it. Every joint is a weak point; keep as few as possible inside a coil.

Which thickness for which job

Wire thickness Resistance per metre Good for
2–3 mm 0.002–0.006 Ω Main connections, outdoor lines, heavy currents
1 mm 0.022 Ω Electromagnets and coils on large batteries, generator windings
0.5 mm 0.09 Ω Galvanometers, relays, small motors, telegraph sounders
0.2–0.3 mm 0.25–0.55 Ω Sensitive detectors, coils needing thousands of turns

(Ω, the ohm, is the unit of electrical resistance. You need it only to compare: less is better for carrying current.)

Measuring thickness without instruments. Wind 20 turns of the wire tightly side by side around a straight stick, push them together, and measure the length of the winding against a ruler (Measurement from Scratch). Divide by 20. Twenty turns of 0.5 mm wire make a band 1 cm wide.

Step 6: Insulate the wire

Bare wire works when the turns cannot touch — a single, spaced layer on a wooden former. For any coil of many turns wound in layers, the wire must be covered. Insulation does not need to be thick: batteries in this book give only a few volts to a few tens of volts.

FROM SIMPLEST TO BEST 1. Bare wire only for single, spaced layers 2. Thread-covered silk or cotton wound in a close spiral 3. Double-covered and varnished two spirals, then shellac, oil varnish or wax A COIL IN LAYERS, CUT THROUGH Covered wire Paper strip between layers Former wood or paper MEASURING THICKNESS 20 turns, pushed tight 0 1 cm 2 cm Width ÷ 20 here 10 mm ÷ 20 = 0.5 mm wooden rule marked in millimetres
Fig. 3 Ways to insulate wire, from simplest to best. Thread-covered and varnished wire is what the first great electromagnets were wound with.

Thread covering (the classic). Wrap silk or fine cotton thread round the wire in a close spiral so that no copper shows. Then wrap a second layer spiralling the other way ("double-covered"). By hand, use a bobbin: hold the wire taut between two pegs and pass a bobbin of thread round and round it, sliding along. Faster: pass the wire through a hollow wooden spindle that carries a bobbin of thread on a disc; turn the disc with a cord from a spinning wheel or The Lathe while you draw the wire slowly through. Then soak the covered wire, or better the finished coil, in melted beeswax or in shellac varnish.

Shellac varnish. Dissolve 1 part (by weight) of crushed lac or shellac flakes in 3–4 parts of strong alcohol from Distillation; it takes a day, stirring now and then. Paint or dip the wire and let it dry for an hour; give it two or three coats. Shellac is a good insulator, sticks well, and dries fast. It also glues coil turns together.

Oil varnish (when there is no lac). Boil linseed oil (from flax seed, see Oils and Pressing) gently for a few hours until it thickens, and melt into it about a quarter of its weight of pine resin (rosin — see Tar, Pitch and Glue). Brush it on thin. It takes a day or two per coat to dry; warmth helps.

Paper between layers. When winding a coil in layers, lay a strip of thin Paper soaked in wax or varnish over each finished layer before winding the next. This stops a turn at the end of one layer touching a turn of the next, where the voltage difference is greatest.

Pitch and tarred cloth. For wires outdoors or buried, wrap them with strips of cloth soaked in hot pitch (Tar, Pitch and Glue), overlapping by half. Heavy, ugly, but keeps water out.

Tip Wax is easy but soft. Beeswax melts at about 63 °C. Coils that carry heavy current get warm; use shellac or oil varnish for them, and keep wax for instruments and coils that stay cool.

How to tell it worked

  • Even thickness. Run the wire between finger and thumb along its length: lumps and thin spots are easy to feel. Wrap tests (20 turns) at several places along a coil should agree.
  • Soft wire bends easily and stays bent. Springy wire needs annealing.
  • Continuity. Connect the wire across a The Battery cell through a compass galvanoscope (see The Electromagnet). The needle should swing. No swing means a break somewhere.
  • Insulation. Wind a few metres of covered wire round an iron bar, or coil it in a bowl of salt water with one end out. Connect one battery terminal to the wire's end and the other through a galvanoscope to the iron bar or the water. The needle should not move. If it does, the covering has a hole: re-varnish.

Note Troubleshooting. Wire snaps at the plate → too big a step between holes, not enough grease, or it needs annealing. Also check for a crack or fold in the rod. Wire comes out scratched or with lines along it → a rough hole, or scale and grit on the wire. Polish the hole, clean the wire. Wire comes out thicker than the hole → it springs back slightly; normal. Measure your wire, not your holes. Thin spots every arm's length → you are pulling in jerks. Use the windlass smoothly. Copper cracks while forging → it was not refined enough (too much oxygen or sulfur), or you worked it too long without annealing.

Dangers

Danger Molten copper and water. A drop of water in a mould, a wet tool, or damp ground under a crucible can turn instantly to steam and spray molten metal. Preheat moulds and tools; keep the casting area dry. Poling also throws up spatter — stand back and wear thick clothing.

  • Snapping wire and flying tongs. Under a windlass, a breaking wire or slipping tongs whip back hard. Never stand in line with the wire under tension; keep your face away from the plate.
  • Wire ends. Cut wire ends are sharp needles and the springy coils jump. Protect your eyes when cutting or uncoiling.
  • Hardening steel. Quenching the draw plate throws out steam; tempering colours come fast. See Blacksmithing and Steel.
  • Fumes. Copper from some ores carries arsenic, which fumes off as white smoke during refining. Work outdoors, upwind; do not breathe it.
  • Alcohol and varnish. Shellac in alcohol and boiling oil are both flammable. Never heat them over an open flame; warm oil varnish in a pot over hot coals, outdoors, with a lid to smother it if it catches.

What this unlocks

How it was first done

The oldest wire, from Egypt and Mesopotamia about 5,000 years ago, was not drawn: it was hammered out, or cut from sheet in thin strips and twisted and rolled round. True drawing through a plate developed later; by about 1120 the German monk Theophilus described iron draw plates with rows of tapered holes for drawing gold, silver and copper wire. By the 1300s wire-drawing in southern Germany used water power to turn the windlasses.

Wire for electricity began in the 1820s. William Sturgeon's first electromagnet (1825) used a few turns of bare copper wire round a varnished iron bar. The American Joseph Henry, around 1828–1831, had the key idea of insulating the wire by wrapping it in silk thread, which let him wind hundreds of turns in layers; by 1831 one of his magnets lifted more than 900 kg. Telegraph lines from the 1840s used thick iron wire on poles; the first undersea cables (1850–51) used copper wire insulated with gutta-percha, a rubbery tree sap from South-East Asia. In 1857 William Thomson (later Lord Kelvin) showed that the conductivity of commercial copper varied by up to a factor of two with purity, which made pure, electrolytically refined copper the standard.