◆ Rebuild

Part 10 · Machines

Springs

A spring stores work when you bend, stretch or twist it and gives it back when you let go. How to make wooden springs, forged leaf springs, wound coil springs and clock mainsprings — and how to harden and temper steel so it springs back instead of staying bent.

Difficulty
●●●●●
Time
An afternoon for a wooden spring; a day for a forged leaf spring; two or three days to draw wire and wind your first good coil springs
Steps from zero
13 prerequisites →

You need first

Steel

This unlocks

Locks and KeysMattresses and UpholsteryThe TypewriterBalances, Steelyards and Weighing MachinesClockwork, Music Boxes and Counting MachinesThe Mechanical ClockWatches and Small ClocksWagons and Carriages
The full path from nothing — 13 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel
  14. Springs

Do them roughly in this order. See it on the tech tree →

Why it matters

A spring is a store of work. Bend it and it pushes back; let go and it returns the effort you put in. Springs return things to place (the The Lathe's spring pole, the valves of a Pumps, a door latch); store power (a The Mechanical Clock mainspring, a bow — Bow and Arrow — or a snare — Hunting and Trapping); cushion shocks under a carriage; hold and press (a pawl against a ratchet — Cranks, Cams and Linkages — or a The Steam Engine safety valve shut); and weigh, because a spring stretches in proportion to the load.

This chapter goes from a green sapling to forged steel, coiled wire and the thin ribbon of a clock spring.

How it works

Stretch is proportional to load

Hang 1 kg on a spring and it stretches, say, 5 mm. Hang 2 kg and it stretches 10 mm; 3 kg, 15 mm. Deflection is proportional to force — this is Hooke's law, and it holds for every spring until you go too far. The force needed for each millimetre of movement is the spring's rate or stiffness (here, 0.2 kg per mm).

The elastic limit, and why steel must be hardened

Every material has an elastic limit. Below it, it springs back fully. Beyond it, it stays bent: the spring takes a set. A good spring is one that can bend a long way before reaching that limit.

Here is the surprise that confuses beginners: soft iron and hardened spring steel are exactly as stiff as each other. A bar of each, the same size, bends the same amount under the same small load. The difference is how far each can go. Soft iron takes a set after bending only a little; hardened and tempered spring steel goes about five to eight times further and still comes back. So you cannot make a better spring by choosing a "stiffer" steel. You make it better by hardening and tempering it so its elastic limit is high — and by giving it the right shape.

Shape decides stiffness

For a flat strip bent like a diving board (a leaf spring):

Stiffness rises with width, with thickness × thickness × thickness, and falls with length × length × length.

So doubling the thickness makes it 8 times stiffer, and doubling the length makes it 8 times weaker. But a thicker strip also reaches its elastic limit after less bending. That is why carts use a stack of thin leaves rather than one thick one: each leaf is thin enough to bend far, and together they carry the load.

For a coil spring made of round wire, the coil is really a long twisted wire:

Stiffness rises with wire thickness to the fourth power, and falls with coil diameter cubed and with the number of coils.

Change Effect on stiffness
Wire twice as thick 16 times stiffer
Coils twice as wide 8 times softer
Twice as many coils 2 times softer (and can stretch twice as far)

A worked example: steel wire 2 mm thick, wound into coils 16 mm across (measured to the middle of the wire), with 10 working coils, has a rate of about 0.4 kg per mm. Keep the coil diameter between 4 and 12 times the wire thickness: tighter than 4 and the wire cracks as you wind it; looser than 12 and the spring buckles and tangles.

Fatigue

A spring that flexes millions of times — a clock's pendulum suspension, a valve spring — can crack even far below its elastic limit. Cracks start at scratches, file marks, rust pits and sharp corners. Every working spring should be smooth, with rounded edges and no nicks, and kept greased.

Leaf springthin leaves stacked and clamped;carts, latches, valves Wooden springsplit ash or yew, tapered to the tip;lathe poles, traps, treadles Spiral (main) springwinds round an arbor inside a barrel Compression springopen coils; pushes backwhen squeezed Extension springcoils wound touching; pulls backwhen stretched Torsion springsqueeze the arms and the coil twists
Fig. 1 The main kinds of spring. Leaf springs bend; coil springs twist their wire as they are pushed or pulled; a spiral spring winds up around its arbor. Wood makes good leaf springs; steel makes all of them.

What you need

Item For Notes
Straight-grained springy wood Wooden springs Ash, yew, hazel, hickory, elm; see below
High-carbon steel, 0.6–1.0% carbon Steel springs See Steel. Test with sparks or quench-and-break first.
Forge, anvil, hammer, tongs Leaf springs, mainsprings See Blacksmithing
Draw plate and draw bench Spring wire See Iron and Brass Wire; for steel, the holes must step down more gently
Mandrel Coiling wire A straight iron or steel rod, with a hole or slot near one end to catch the wire, and a crank
Quench pot Hardening Oil or melted animal fat, at least 10 cm deep over the work, with a lid
Sand tray Tempering An iron pan of dry sand on the fire
Files, sandstone, fine sand Finishing Remove every scratch before hardening
Weights Testing Stones or bags of sand weighed on a balance (Measurement from Scratch)

Where to find it

  • Springy woods. Yew is the finest (see the materials list; its leaves and seeds are poisonous). Ash is tough and forgiving; hazel gives many straight rods; hickory, elm, osage orange and hornbeam are all good. Test: a dry stick as thick as your thumb should bend and spring straight back with a snap.
  • Spring steel. If you have any old steel — a broken file, a saw blade, a cart spring — it is likely good spring steel; spark-test it (Steel). From scratch, make blister steel by carburising thin iron and fold it until even. Spring steel needs to be clean: a slag streak in a spring is a crack waiting to happen, so use your best, most refined steel.
  • Brass and bronze. Hammered cold, brass and tin bronze become springy ("spring-hard"). They cannot be hardened by heat, but they do not rust, which suits light springs in damp places. Ancient brooch pins were coiled from hammered bronze wire. See Bronze and Zinc and Brass.

Method 1: Wooden springs

Wood is the easiest spring and good enough for a lathe pole, a trap, a treadle return, a door closer or the spring of a hand-operated press.

  1. Split, don't saw. Cleave a stave from a straight, knot-free log so the grain runs the whole length. A sawn piece with grain running out of its side will snap.
  2. Shape it to a flat, slightly tapering strip. As a rule, make it at least 40–50 times as long as it is thick if it must bend a lot: a 1 m spring should be no more than 2–2.5 cm thick where it is held. Thinner = bends further safely; wider = stronger.
  3. Taper towards the tip so the whole length bends evenly. A strip of even thickness bends most at its root and breaks there.
  4. Keep the "back" untouched. The side that will be stretched (the outside of the curve) should be one unbroken growth ring if possible, as in a bow. Never cut across the grain on that face.
  5. Season it for a few weeks if you can; green wood springs but slowly loses its spring ("follows the string"). A lathe pole is the exception — use it green and replace it when it tires.
  6. Grease or oil it to keep moisture steady.
  7. Load it gradually the first time, bending a little further each day until it reaches working bend.

A wooden spring carries roughly a quarter of its length as safe tip movement when built to the proportions above. If you need more movement, make it longer, not thicker.

Method 2: A forged leaf spring

For latches, traps, tongs, shears that open by themselves, pump valves and cart suspension.

  1. Forge the strip from high-carbon steel, to the size and curve you need. Forge it at orange to bright cherry heat (900–1,000 °C) and stop hammering when it falls to dull red — hammering spring steel cold cracks it.
  2. Taper it towards the free end (thinner, or narrower like a triangle seen from above) so it bends evenly along its length.
  3. Normalise. Heat to cherry red and let it cool in still air. Do this three times; it refines the grain.
  4. File and polish. Remove all hammer marks and scale. File along the length, never across: a cross-wise scratch is where the spring will crack. Round all the edges slightly. Finish with sandstone and wet sand.
  5. Bend it to shape now, while soft. Bend a little more than the finished curve, because it will open slightly in hardening.
  6. Harden. Heat it evenly to cherry red (about 800 °C) — the magnet just stops sticking — and plunge it into oil or melted fat warmed to about 50 °C. Move it up and down. Oil is gentler than water and cracks far fewer springs.
  7. Temper to blue. Polish a strip bright. Lay the spring in a tray of hot sand and watch the colours run: pale straw, straw, brown, purple, dark blue (about 290–300 °C). For a spring, the whole piece should reach an even dark blue, then cool in air. See the colour table in Steel.
  8. Or "blaze it off". The old spring-maker's way: dip the hardened spring in oil or fat, hold it over the fire until the oil catches and burns off with a flame, let it go out, dip again and repeat — three times for a thin spring. The burning oil brings the whole piece to about the right tempering heat at once, even where it is too dark to see colours.

A cart leaf spring is a stack of such leaves. The top leaf (the main leaf) is longest and has an eye rolled at each end; each leaf below is shorter by an equal step, so the stack is shaped like a long thin triangle. All are curved alike, then clamped together at the middle with a U-shaped band or bolt. A typical light cart spring has 4–6 leaves, each 5–6 mm thick and 4–5 cm wide, the main leaf about 90 cm long.

Method 3: Coil springs

Wire caughtin a hole in the mandrel Coils at an even pitchgap = squeeze ÷ number of coils Mandrel10–20% smaller than the inside size Crankturn slowly Grooved guide blockpull back hard; slide it along annealed wire 1. Test coilinside size Wind a few turns, let go,measure; adjust the mandrel 2. Harden Cherry red (~800 °C), thenstraight into warm oil 3. Temper On hot sand until dark blue(290–300 °C), or blaze off
Fig. 2 Winding a coil spring. Annealed wire is caught in a slot in the mandrel and guided on at an even pitch while the mandrel is cranked. The spring is then hardened in oil and tempered blue.

Make the wire

Draw steel wire as in Iron and Brass Wire, but anneal it often — heat to dull red and cool slowly in wood ash after every 2–3 holes — step down gently, and keep it greased with tallow. Wire drawn hard through the last few holes without a final anneal is already springy: small springs wound from it cold need only a low stress-relief heat (step 6 below).

Wind the spring

  1. Choose the mandrel. Wire springs open out a little when released, so use a mandrel about 10–20% smaller than the inside diameter you want. Find the right size by trial on a short test coil.
  2. Anneal the wire (unless you are using hard-drawn wire). Soft wire winds easily and holds its shape.
  3. Anchor the end. Push the wire through a hole or slot near the end of the mandrel, or bend it round a pin.
  4. Wind it. Hold the wire with a leather pad or a wooden block with a groove, pulling back firmly to keep it tight, and turn the mandrel slowly with a crank. The mandrel can be held in a The Lathe, in a vice with a crank on its end, or simply in two notched posts.
    • Compression spring (pushes back when squeezed): guide the wire along so the coils are evenly spaced. The gap between coils must be greater than the distance the spring will be squeezed, divided by the number of coils. A thin rod laid between the turns as you wind, or a groove cut in the guide block, keeps the spacing even.
    • Extension spring (pulls back when stretched): wind the coils touching each other, then bend up the last half-turn at each end into a loop or hook.
    • Torsion spring (twists): close-wound, with both ends left long and straight as arms.
  5. Finish the ends. Cut off. For compression springs, close the last coil at each end flat against its neighbour and file it flat, so the spring stands square.
  6. Heat-treat.
    • Annealed wire: harden by heating the whole spring evenly to cherry red — in a covered iron box in the fire, or on an iron plate, so the thin wire does not burn — then drop it into oil. Temper to dark blue in hot sand, or blaze off as above.
    • Hard-drawn wire: do not harden. Just heat gently to about 250–300 °C (until a clean bit of wire turns brown to blue, or a pinch of sawdust on it scorches) and cool. This relieves the strain of winding so it keeps its shape.

Method 4: A clock mainspring (advanced)

A mainspring is a long, thin, hardened ribbon coiled in a drum (the barrel), with its inner end hooked to a central shaft (the arbor) and its outer end hooked to the barrel. Winding the arbor coils the spring tight; the barrel then turns slowly as it unwinds, driving the clock's gears.

  1. Forge a ribbon of your finest steel — for a small clock about 0.3–0.5 mm thick, 12–20 mm wide and 60–100 cm long — finishing by cold hammering with a polished hammer on a polished anvil (annealing often) or by rolling (Sheet Metal and Rolling). It must be the same thickness everywhere; a thin spot breaks first. Smooth and round the edges.
  2. Harden it coiled loosely in a closed box, all at once, and quench in oil; temper to blue evenly; polish both faces lengthways.
  3. Soften just the ends with a hot iron and bend the inner end into a hook-eye for the arbor, the outer into a loop for the barrel hook.
  4. Proportions. The arbor should be at least 25 times as thick as the spring — wound tighter than that, it breaks. The coiled spring should fill about half the space between arbor and barrel wall, leaving the other half free for it to unwind into.
  5. Grease lightly and wind it into the barrel with a winding tool (a clamp and crank), never by hand alone.

A fully wound mainspring pushes much harder than a nearly run-down one. Clockmakers evened it out with a cone-shaped pulley (a fusee) — see The Mechanical Clock.

How to tell it worked

  • The set test. Measure the spring's length (or the height of its curve), load it to its full working movement ten times, and measure again. It must come back to within about 1–2%. A spring that shortens or flattens a little the first few times and then stays the same is fine ("settled"); one that keeps getting shorter is too soft — re-harden and temper less (purple instead of blue).
  • The rate test. Hang known weights from it and measure the stretch. Equal weights should give equal stretches. Mark the stretches on a board behind it and you have a spring balance.
  • The ring and fatigue tests. A good spring rings when tapped and snaps back lively (a dull thud means soft iron). Worked a few thousand times on a treadle or waterwheel, a sample should not crack.

Note Troubleshooting. Spring takes a set (stays bent) → not hardened (not enough carbon, or not hot enough when quenched), or tempered too far (grey-blue or beyond). Re-harden and temper only to dark blue or purple. Or it is simply worked too far: make it longer, thinner, or with more coils. Snaps suddenly → tempered too little (still brittle), a scratch or file mark across it, a slag streak in the steel, or a sharp bend at an eye. Polish lengthways, round the bends, temper fully to blue. Cracked in the quench → water used instead of oil, or overheated. Use oil, cherry red only. Coil spring is too stiff or too soft → use the table above: change the number of coils first (easy), then the coil diameter, and only then the wire size. Compression spring bows sideways → too long for its width (more than about 4 times longer than its diameter); fit it over a rod or inside a tube. Wire cracks while winding → mandrel too small, or wire not annealed.

Dangers

Danger Stored springs release with violent force. A clock mainspring that slips while winding or unwinding unwinds in an instant and can slice hands to the bone or strike the face. Always let a mainspring down slowly with a key held firmly, wear thick gloves, and keep it caged. A large leaf or coil spring under load — a cart spring being clamped, a press spring — can throw its clamp or itself across the room. Never stand in line with a compressed spring, and release load with a screw or lever, never by knocking out a pin.

  • Quench-oil fires. Use a deep pot with a lid at hand, outdoors. Blaze off over the forge, away from fuel, a little oil at a time.
  • Flying ends. Wire whips if it slips from the guide; protect your eyes.
  • Brittle springs shatter. Test new springs behind a board or wrapped in cloth.

What this unlocks

With springs you can build a spring-driven The Mechanical Clock, the valves of pumps and Bellows to Air Compressors, the safety valve of the The Steam Engine boiler, the spring returns and tension discs of the The Sewing Machine, locks, spring balances for weighing (Balances, Steelyards and Weighing Machines), and the suspension of Wagons and Carriages, railway cars and the The Bicycle. Thin hairsprings let a balance wheel keep time in a watch (Watches and Small Clocks). Coil springs made to standard sizes become one of the first Precision and Interchangeable Parts.

How it was first done

Bent-wood springs are as old as the bow and the snare. Bronze Age brooches (fibulae) from about 1300 BC have a pin with a coiled spring of hammered bronze wire, the ancestor of the safety pin. The Greek engineer Ctesibius of Alexandria, around 250 BC, is said to have experimented with springs of hammered bronze. Steel springs appear in European locks in the Middle Ages, and the coiled mainspring made portable clocks possible in the 1400s; the oldest surviving spring-driven clock is usually dated to around 1430. Robert Hooke announced the law of springs in 1676 as a scrambled Latin anagram and revealed it in 1678: "ut tensio, sic vis" — "as the extension, so the force" — and used it in the balance spring for watches. Steel leaf springs under carriages spread in the 1700s, and Obadiah Elliott patented the elliptic carriage spring in England in 1804.

Source: content/entries/mechanics/springs.md