◆ Rebuild

Part 3 · Metals

Tungsten and Filament Wire

Tungsten melts at 3,422 °C, hotter than any furnace you can build, so it is never melted at all. You dissolve it out of its ore, purify it as a yellow oxide, turn that to metal powder in a stream of hydrogen, press and sinter the powder into bars by passing a huge current through them, then hammer and draw the bars hot into wire finer than a hair — the filament of the electric lamp. Mixed with carbon and cobalt, the same powder makes tungsten carbide, the tool tip that cuts hardened steel.

Difficulty
●●●●●
Time
Weeks to set up the chemistry and furnaces; two to three days from ore to a sintered bar; days more to swage and draw it to wire
Steps from zero
27 prerequisites →

You need first

Finding and Identifying OresHydrogen, Oxygen and GasesIron and Brass Wire

This unlocks

Fused Quartz and Halogen LampsMolybdenumPowder Metallurgy
The full path from nothing — 27 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Lime
  14. Fermentation
  15. Lye and Potash
  16. Glass
  17. Bellows
  18. Copper Smelting
  19. Iron (the Bloomery)
  20. Laboratory Glassware
  21. Blacksmithing
  22. The Battery
  23. Steel
  24. Electrolysis
  25. Copper Wire
  26. Iron and Brass Wire
  27. Hydrogen, Oxygen and Gases
  28. Tungsten and Filament Wire

Do them roughly in this order. See it on the tech tree →

Why it matters

The carbon filament lamp (The Light Bulb) is dim, reddish and short-lived, because carbon boils away if run hotter than about 2,100 °C. A tungsten filament runs at 2,500–2,800 °C, so it gives about three times the light for the same electricity, whiter, for a thousand hours. Tungsten also makes the hot filaments and targets of X-ray tubes and radio valves, electrodes for arc Welding, contacts that do not weld together in switches and car ignitions, heating elements for hydrogen furnaces, and the anvils of the presses that make synthetic diamond.

As tungsten carbide, it is the hardest everyday tool material after diamond: lathe tips that cut steel three to five times faster than high-speed steel (Machine Tools, Alloy and Stainless Steels), rock-drill bits for Mining and Tunnelling and Tunnels and Rock Drilling, and wire-drawing dies that last a hundred times longer than steel (Iron and Brass Wire).

Be honest with yourself: this is one of the hardest chapters in the book. It needs good chemistry, a steady supply of hydrogen, a large transformer and a team. The first section gives the easiest route to a working lamp: a pressed-paste filament that needs no drawing at all.

How it works

You cannot melt it. No crucible survives 3,422 °C. So tungsten is made by powder metallurgy (Powder Metallurgy): make the metal as a fine powder, squeeze the powder into a bar, and heat the bar until the grains weld together without melting (sintering).

Carbon will not do. Charcoal reduces tungsten oxide to metal (Alloy and Stainless Steels does it for steelmaking), but some carbon stays behind as carbide and makes the metal brittle. Hydrogen takes the oxygen away as water vapour and leaves pure metal:

tungsten oxide + hydrogen → tungsten + water. 1 kg of oxide gives 793 g of metal and needs about 290 litres of hydrogen, in practice 3–5 times that flowing through.

The bar heats itself. A pressed bar of powder conducts electricity. Clamp it between two copper jaws in hydrogen and pass a very large current: it glows white, reaches about 3,000 °C and shrinks as it sinters into solid metal.

Hot hammering makes it ductile. Sintered tungsten is brittle at room temperature: its grains are round and their boundaries are weak. Hammered and drawn hot, the grains are stretched into long fibres, like the grain in wood, and the wire becomes tough enough to bend and coil cold. This was William Coolidge's great discovery of 1909–1910. If wire is heated too long it recrystallises back into round grains and becomes brittle again — which is why an old lamp filament snaps when you tap the bulb.

What you need

Item For See
Ore concentrate, 60–70% tungsten oxide Feed Below, Finding and Identifying Ores
Soda ash, Hydrochloric Acid, ammonia water Dissolving and purifying Soda Ash and Baking Soda, Ammonia
Iron pots, pottery or glass vessels, filter cloths Chemistry Laboratory Glassware
Hydrogen, 1–2 cubic metres a day, dried Reduction and sintering Hydrogen, Oxygen and Gases
Hydrogen tube furnace, 800–1,000 °C Making powder Below
A hydraulic press, 20–50 tonnes, and a hardened split steel mould Pressing bars Hydraulic Presses and Rams
A transformer giving 1,000–2,000 A at 10–15 V, with a way to raise the current slowly Sintering The Transformer
Water-cooled bell jar with copper clamps Sintering in hydrogen Below
Rotary swager and a hydrogen furnace at 1,200–1,600 °C Swaging Below, Machine Tools
Draw bench, tungsten carbide dies and diamond dies, colloidal graphite Drawing Iron and Brass Wire, Industrial Diamond and Hard Abrasives
Cobalt powder Carbide Nickel and Cobalt

Where to find it

  • Wolframite — dark brown to black, very heavy, in flat bladed crystals with one perfect cleavage, in quartz veins round granite with tin ore. Full description in Alloy and Stainless Steels.
  • Scheelite — calcium tungstate. White, cream, grey or pale yellow-brown, with a greasy-glassy shine; looks like quartz or calcite but is far heavier (about 6 times water, against 2.7 for quartz) and too hard to scratch with a copper coin yet scratched by steel. Found where granite has baked limestone (skarn — a dark rock of garnet and pyroxene at granite–limestone contacts) and in quartz veins. Its best test: under short-wave ultraviolet light in the dark it glows a bright sky blue-white. Prospectors searched outcrops at night with a mercury arc lamp in a quartz tube behind a dark filter (Arc Lamps, Neon and Fluorescent Lights).

Concentrating. Crush the ore to sand size and pan or jig it (Finding and Identifying Ores, Mining and Tunnelling): both minerals are so heavy that they stay in the pan with the tin stone. Wolframite is weakly magnetic and tin stone is not, so a strong electromagnet (The Electromagnet) drawn over the dry concentrate pulls the wolframite out. Aim for a concentrate that is mostly heavy dark (or white) grains, with little quartz.

Step 1: Pure tungstic oxide

1. Concentrate wolframite or scheelite 2. Fuse with soda leach, precipitate, purify 3. Tungstic oxide pure lemon yellow 4. Reduce in hydrogen 600–1,000 °C → grey powder H₂ 5. Press a bar 2–3 tonnes per cm² 6. Sinter by current about 3,000 °C, in hydrogen 7. Swage, then draw hot carbide, then diamond dies 8. Coil the filament on a steel mandrel, then dissolve the mandrel in acid
Fig. 1 From ore to filament. Ore is dissolved and purified to yellow oxide, reduced to grey powder in hydrogen, pressed into a bar, sintered by its own current, swaged hot and drawn through carbide and diamond dies, then coiled.
  1. Fuse. Grind wolframite concentrate fine. Mix it with 1–1.2 times its weight of soda ash and heat it in an iron pot to a bright red (800–900 °C) for about an hour, stirring with an iron rod, until it has melted and stopped bubbling. The tungsten becomes sodium tungstate, which dissolves in water; iron and manganese stay as insoluble oxides. (Scheelite can skip this: boil it, finely ground, in strong hydrochloric acid for several hours, stirring, and go straight to step 4.)
  2. Leach. Cool, break up the cake, and boil it in water. Let it settle, pour off the clear liquid, and boil the residue twice more with fresh water. Filter the combined liquid through cloth.
  3. Precipitate. Pour the hot sodium tungstate solution slowly, stirring, into an equal volume of hot strong Hydrochloric Acid. Yellow tungstic acid falls out. Boil for half an hour, let it settle, pour off the liquid.
  4. Wash the yellow mud with hot water slightly sour with acid, five or six times, until the washings leave almost nothing when a drop is dried on glass.
  5. Purify through ammonia. Stir the wet tungstic acid into warm Ammonia water until it dissolves; silica and other dirt stay behind. Filter. Evaporate the clear liquid slowly: white crystals of ammonium paratungstate form — the purest form of tungsten you can make. Crystallise twice for lamp wire.
  6. Calcine. Heat the crystals in a clean pottery dish to a dull red (600–800 °C) for an hour. Ammonia and water drive off, leaving a bright lemon-yellow powder: pure tungstic oxide.

Step 2: Reducing to powder in hydrogen

The hydrogen tube furnace

600–700 °C 850–1,000 °C cooling zone loading end Iron or fireclay tube 5–8 cm bore, 1–1.5 m long heating winding Boats pushed through yellow oxide → brown → grey metal powder Cool in hydrogen before opening Hydrogen in Drying tower quicklime Burn-off flame
Fig. 2 The hydrogen tube furnace. Boats of oxide are pushed in from the loading end through a cooler and a hotter zone; dry hydrogen flows the other way and is burnt as it leaves. The boats cool in hydrogen before they come out.

A straight tube of iron, nickel-steel or glazed fireclay, 5–8 cm across and 1–1.5 m long, lying horizontally through a furnace that heats its middle 50–80 cm. Heat it with charcoal or gas in a brick setting, or better with an electric winding of iron-chromium or nickel-chromium wire round a fireclay tube (Electric Kettles, Irons, Heaters and Cookers). Fit each end with a removable cap sealed with a gasket.

  • Hydrogen in at the outlet end — the gas flows against the direction the boats travel, so the freshest, driest gas meets the most nearly finished powder.
  • Hydrogen out at the loading end, through a pipe to a small flame burning at a safe distance. The flame shows the gas is flowing and burns off what is left.
  • Dry the hydrogen first, through a tower of lumps of quicklime (Lime) or a wash-bottle of strong Sulfuric Acid. Water in the gas slows the reduction and coarsens the powder. Hydrogen from splitting water (Electrolysis) is the cleanest.
  • Boats: shallow trays of iron or nickel sheet, 25–30 cm long, holding the oxide in a layer 1–2 cm deep.

Reducing

  1. Purge. Before heating, drive all air out of the tube — with nitrogen or carbon dioxide if you have it, or with at least ten tube-volumes of hydrogen. Collect a test tube of gas from the outlet and do the pop test (Hydrogen, Oxygen and Gases): only when it burns quietly is the tube free of air. Then light the outlet flame.
  2. First stage. Push the boats into the hot zone at 600–700 °C for 2–4 hours. The yellow oxide turns chocolate brown (a lower oxide).
  3. Second stage. Raise the furnace to 850–1,000 °C for another 3–5 hours. Lower temperatures make finer powder (good for wire); higher make coarser powder.
  4. Cool in hydrogen. Pull the boats into the cold end of the tube and let them cool completely under flowing hydrogen. Hot fine tungsten powder catches fire in air.
  5. Check. The powder should be an even dull grey, with no yellow or brown, and astonishingly heavy. Weigh the boat before and after: a complete reduction loses 20.7% of the oxide's weight.
  6. Sieve through fine silk or brass gauze and store in sealed jars.

Step 3: Pressing and sintering the bar

Hydrogen out burnt at a flame Iron bell water jacket Pressed bar white-hot, about 3,000 °C; shrinks about 15% Flexible strap lets the bar shrink Hydrogen in dry Copper clamp water-cooled water out Copper clamp water in Transformer 1,000–2,000 A at 10–15 V
Fig. 3 The sintering bell. The pressed bar hangs between water-cooled copper clamps inside an iron bell filled with flowing hydrogen. Current is raised slowly until the bar glows white and shrinks into solid metal.
  1. Press. Fill a hardened, polished split steel mould with a cavity about 6 × 6 × 150 mm with powder, level it, and press it from the long side in a hydraulic press at 2–3 tonnes per cm² — 20–30 tonnes on this mould. Open the mould sideways and lift the bar out on a flat plate. It is about 60% solid, weighs about 60 g, and breaks like chalk.
  2. Presinter. Slide it on a boat into the hydrogen furnace at 1,100–1,200 °C for 30–60 minutes. Now it can be handled.
  3. Treat (sinter by current). Clamp the bar upright between two water-cooled copper clamps inside an iron bell with a water jacket, standing on a base with a gasket. The bottom clamp hangs on a flexible strap so the bar can shrink without breaking. Flush with hydrogen as above.
  4. Find the fusing current. With a test bar from the same batch, raise the current slowly until the bar melts through. Note the current. Your working current is 88–92% of it — roughly 1,000–1,500 A for a 6 mm bar.
  5. Sinter. Raise the current to the working value over 10–15 minutes, hold it for 15–20 minutes, then turn it down and let the bar cool in hydrogen. The bar shrinks by about 15% in length, its surface turns bright and slightly crystalline, and it reaches 90–95% of full density.

A good bar rings when tapped, is the same thickness all along, and shows a fine grey crystalline break when a scrap end is snapped.

Step 4: Swaging and drawing to wire

Rotary swager

A rotary swager is a spinning steel head holding two hardened dies with a tapered groove between them. As the head spins, the outer ends of the dies run over a ring of hardened rollers, which slam the dies together 2,000–4,000 times a minute. The bar is pushed into the groove and hammered evenly all round. Build it on a lathe-type spindle (Machine Tools) with hardened tool-steel dies; you need a set of dies, each 10–15% smaller in area than the last.

  1. Heat the bar in a hydrogen tube furnace standing right beside the swager, to 1,500–1,600 °C (dazzling yellow-white) for the first passes. Look only through dark welding glass.
  2. Swage: pull it from the furnace and push it through the swager in one movement, within seconds. Reheat between passes.
  3. Lower the heat as it thins — down to about 1,200 °C (bright orange) by the time it is 1 mm.
  4. Take it from 6 mm square to about 1 mm round in 20–30 passes. By then it has become fibrous and can be bent a little cold without breaking.

Drawing

  1. Coat the wire in colloidal graphite — the finest graphite powder settled out in water (by settling) mixed with a little gum — and dry it.
  2. Draw hot. Pass the wire through a small gas flame or electric heater just before the die, to 600–900 °C (dull to bright red), and through a die that is heated too. Draw with a slowly turning drum (Iron and Brass Wire).
  3. Dies. Use tungsten carbide dies (below) down to about 0.3 mm; finer than that, diamond dies (Industrial Diamond and Hard Abrasives). Each die reduces the area by 15–20% at first, 8–12% for the finest sizes. The temperature comes down as the wire thins.
  4. Size by weight. Fine wire is too thin to measure. Weigh a 200 mm length: tungsten weighing 19.3 g per cm³, a 0.03 mm wire weighs 2.7 mg per 200 mm; 0.05 mm weighs 7.6 mg.
  5. Clean off the graphite by drawing the wire through hot Lye and Potash solution, or by passing a current through it in lye.

The tungsten filament

Lamp Wire diameter Length
230 V, 60 W about 0.03 mm about 60–70 cm
230 V, 100 W about 0.04 mm about 80–90 cm
120 V, 60 W about 0.045 mm about 45–50 cm
6 V, 3 W torch bulb about 0.04 mm about 2–3 cm

These are approximate; test and adjust.

  1. Coil it. A straight filament 70 cm long would fill the bulb and lose heat to the gas. Wind it tightly on a steel mandrel wire two to three times its own diameter, the turns spaced about one wire-thickness apart, by turning the mandrel slowly in a hand lathe and guiding the tungsten with a weighted feed.
  2. Set the coil by heating it on its mandrel to about 1,200 °C in hydrogen for a few minutes, so it keeps its shape.
  3. Dissolve the mandrel in warm Hydrochloric Acid. Acid eats the iron and leaves the tungsten untouched. Rinse well and dry.
  4. Mount the coil on two lead-in wires and one or two thin support hooks, and seal it into the bulb (The Light Bulb). Lamps under about 25 W are pumped to a hard vacuum; bigger lamps are filled with argon with a little nitrogen at about 0.8 of atmospheric pressure (Liquid Air, Nitrogen and the Noble Gases), which slows the tungsten from boiling away so the filament can run hotter. A speck of red Phosphorus on the filament mops up the last traces of oxygen and water when the lamp is first lit.
  5. Flash it: run the first lamp of a batch on half voltage for a minute, then full.

The easier route: the pressed-paste filament

Before ductile wire, lamps were made from squirted filaments, and so can yours.

  1. Mix the finest tungsten powder with a thick binder — sugar syrup, gum arabic or dextrin paste — into a paste as stiff as putty.
  2. Force it through a tiny hole, 0.05–0.15 mm across, drilled in a diamond or a ruby (Synthetic Gems), with a small screw press. A thread comes out like a hair.
  3. Dry the threads straight on a frame, then bake them in hydrogen at red heat to char and drive off the binder.
  4. Sinter each one by passing current through it in hydrogen, raising it slowly to a white glow.
  5. Mount these brittle filaments as several hairpins in series in a vacuum bulb, and never jolt the lamp.

They gave about three times the light of carbon, but broke easily when the lamp was knocked. It is a real working lamp, and it needs no swager or diamond dies.

Tungsten carbide tip

  1. Carburise. Mix tungsten powder with 6.1% of its weight of the purest carbon — lampblack (Lampblack and Carbon Black) or sugar charcoal — in a ball mill. Heat it in graphite boats in hydrogen at 1,400–1,600 °C for an hour or two. It becomes tungsten carbide powder, dark grey.
  2. Mill with cobalt. Put 94 parts carbide and 6 parts cobalt powder (Nickel and Cobalt) in a steel jar half full of hardened steel or carbide balls, cover with spirit or paraffin oil, and roll it for 2–4 days. The cobalt must coat every grain.
  3. Press. Dry the mix, stir in 1–2% paraffin wax dissolved in petrol as a binder, and press into blanks at 1–2 tonnes per cm².
  4. Presinter in hydrogen at 800–900 °C. The wax burns off, and the blank is now like hard chalk: shape it now, with files and saws, making it 20% oversize every way.
  5. Sinter at 1,400–1,500 °C for about an hour, in hydrogen in a carbon-tube or molybdenum-wound furnace (Electric Kilns and Furnaces), the blanks packed in alumina powder. The cobalt melts, wets the grains and pulls them together: the blank shrinks about 18–20% each way into a grey, dense, enormously hard tip.
  6. Braze it into a pocket milled in a medium-carbon steel shank with copper or brass under borax (Soldering and Brazing), a thin copper shim between to take the strain. Cool slowly, buried in ash.
  7. Grind it with a green silicon carbide wheel (Precision Grinding), finish on a diamond lap. Give it a strong, blunt edge — little or no top rake — because carbide is brittle.

A good tip scratches glass and a hardened file easily, takes no mark from a file, and weighs about 15 g per cm³ — twice as heavy as steel. Run carbide at 3–5 times the cutting speed of high-speed steel, with a rigid lathe and no chatter.

How to tell it worked

  • Oxide is clear lemon yellow; green or grey means it is impure or partly reduced.
  • Powder loses exactly 20.7% of the oxide's weight and shows no colour.
  • Sintered bar: shrunk about 15% in length, rings when tapped.
  • Wire: weight per 200 mm matches the table, it bends round a pencil without cracking, and it is bright after cleaning.
  • Lamp: a 60 W lamp should be far brighter and whiter than a carbon lamp of the same power, and should not blacken the bulb within the first hours.

Note Troubleshooting. Powder has blue or brown streaks → not fully reduced. Longer time, drier hydrogen, thinner layer. Bar breaks on pressing → powder too coarse or too dry; add a few drops of glycerine in alcohol per 100 g and press again. Bar melts through when treating → current too high or raised too fast; sinter at 88% of the fusing current. Bar splits lengthways on the swager → too cold, or reduced too much per pass. Hotter, smaller steps. Wire snaps at the die → die cracked or rough, not hot enough, or too much reduction. Inspect the die under a lens. Filament blackens the bulb fast → air or water in the bulb, or run too hot. Pump harder, add phosphorus getter, check the voltage. Carbide tip crumbles → too little cobalt, poorly milled, or underheated. Mill longer and sinter hotter.

Dangers

Danger Hydrogen explodes. Mixed with air in almost any proportion between 4% and 75% it detonates from a spark. Every furnace, bell and pipe must be purged of air before heating and kept under a slight positive flow so air cannot leak in. Test with the pop test every time. Never open a hot furnace full of hydrogen; burn the exhaust gas at a flame well away from the operator. Work in a high, airy building, because leaking hydrogen gathers under the roof.

Danger Carbide and cobalt dust damage the lungs for life ("hard metal disease"), and cobalt causes asthma and skin allergy. Mill and handle powders wet or in closed vessels, grind carbide wet, wear a damp cloth mask at the least, and never sweep dry.

  • Pyrophoric powder. Fine hot tungsten, cobalt and carbide powders can burst into flame in air. Cool under hydrogen.
  • Glare. A treating bar or swaging furnace at 1,500–3,000 °C damages eyes. Look only through dark welding glass. Ultraviolet lamps for prospecting burn eyes and skin in minutes.
  • Heavy currents of a thousand amperes heat clamps, cables and rings on fingers red-hot instantly. Take off all metal from hands; switch off before touching.
  • Hot soda melts, acids and ammonia burn skin and eyes; ammonia fumes choke (Acids, Bases and Testing, Ammonia).

What this unlocks

Bright electric light (The Light Bulb, Dry Cells and Electric Torches, Arc Lamps, Neon and Fluorescent Lights for fluorescent-tube filaments); hot-cathode X-ray tubes and The Vacuum Tube heaters; tungsten electrodes for arc Welding; carbide tools for Machine Tools and Precision Grinding, rock drills for Mining and Tunnelling, and carbide dies for Iron and Brass Wire and Presses, Punches and Dies; and the press anvils of Industrial Diamond and Hard Abrasives.

How it was first done

In 1781 the Swedish chemist Carl Wilhelm Scheele got a new acid out of the heavy white mineral then called tungsten ("heavy stone" in Swedish) — today's scheelite. In 1783 the Spanish brothers Juan José and Fausto Elhuyar, at Bergara, made the same acid from wolframite and reduced it with charcoal to the first metallic tungsten. In 1868 Robert Mushet in England made tungsten tool steel.

In 1904 Alexander Just and Franz Hanaman in Budapest patented the first tungsten filament lamps, made from squirted and sintered paste; they went on sale around 1906. In 1906–1910 William Coolidge at General Electric's laboratory in Schenectady, New York, worked out pressing, current sintering, hot swaging and hot drawing through diamond dies, and ductile tungsten wire went into lamps from 1911. Irving Langmuir at the same laboratory made the gas-filled lamp with a coiled filament in 1913. Around 1917 Aladar Pacz found that a trace of potassium and other additives made filaments that did not sag. In 1923 Karl Schröter at the Osram lamp company in Germany invented cemented tungsten carbide, sold by Krupp from 1926 under the name Widia, from wie Diamant, "like diamond".

Source: content/entries/metals/tungsten.md