Part 2 · Earth and Fire
Quarrying and Cutting Stone
How to get big, sound blocks of stone out of the ground by following its natural beds and splitting it with wedges, then dress the blocks square and move them with levers, sledges and rollers. Stone lasts for thousands of years; this is how you get it.
- Difficulty
- ●●●●●
- Time
- Hours to split a small block; days to weeks for a large one; a day to dress a good building stone by hand
- Steps from zero
- 2 prerequisites →
The full path from nothing — 2 steps before this one
- Stone Tools
- Simple Machines
- Quarrying and Cutting Stone
Do them roughly in this order. See it on the tech tree →
Why it matters
Stone does not rot, burn or get eaten by insects. Walls, foundations, bridges, harbours, millstones, troughs, querns, kerbs and steps made of stone outlast the people who build them by centuries. Stone is also the raw material for Lime, Portland Cement, Mortar and Concrete and road metal for Roads and Bridges.
Picking up loose stones is enough for a field wall. But to build squared walls, arches, lintels and millstones, you need blocks of a chosen size and shape, without hidden cracks. That means taking stone from the living rock — quarrying — and then dressing it (shaping its faces). The method is almost the same everywhere: find the natural planes of weakness, split along them with wedges, lever the block free, and square it with chisels.
This chapter leads to Stone Masonry, Foundations and Floors, Arches, Vaults and Domes and, underground, to Mining and Tunnelling.
How it works
Stone has a grain
Rock is not equally strong in every direction. Most rock is crossed by natural planes of weakness:
- Bedding planes — in sedimentary rock (sandstone, limestone, slate's parent shale), the boundaries between the layers it was laid down in. Stone splits along beds far more easily than across them.
- Joints — natural cracks, usually at roughly right angles to the bedding, that divide the rock into rough blocks. They come in sets running in two or three directions.
- Rift and grain — even granite, which has no layers, splits more easily in one direction (the rift), less easily in a second (the grain), and worst in the third (the hardway). Quarry workers find them by test splits and by watching how weathered boulders break.
A good quarry face is one where beds and joints already outline blocks of a useful size. You only have to cut the one or two sides that nature did not.
Wedges turn hammer blows into huge pressure
A wedge is a ramp driven by blows (see Simple Machines). A row of wedges in a line of holes or a groove multiplies the force of each hammer blow many times and concentrates it on a line. Rock is strong when squeezed but weak when pulled apart — its strength in tension is only about a tenth of its strength in compression. A row of wedges pulls the rock apart along a line, and a crack runs from wedge to wedge.
Fresh stone is softer
Newly quarried limestone and sandstone contains moisture called quarry sap. While it is "green", it cuts much more easily. As it dries over weeks and months, minerals deposited from the sap harden its surface. So: quarry, split and dress soft stone soon after it comes out, and do not let wet green stone freeze — water in its pores expands and cracks it.
What you need
| Item | Details |
|---|---|
| Wedges | Hardwood (oak, ash, hornbeam): 15–25 cm long, 4–6 cm thick at the head, tapering to 1 cm. Later iron: 10–20 cm long, 2–3 cm thick. Make many — 10 to 30. |
| Plug and feathers | For iron splitting in drilled holes; see Method 2 and Blacksmithing |
| Hammers | A 1–2 kg hammer for drilling and wedges; a 4–6 kg sledge for big wedges. Hard hammerstones of basalt or quartzite before you have iron. |
| Picks | Pointed iron pick or antler pick for channelling soft stone |
| Hand drill (jumper) | An iron or steel bar 2–2.5 cm thick, 30–60 cm long, with a chisel-shaped, hardened tip; see Steel |
| Chisels | Point (pointed), claw or toothed, and flat chisels of hardened steel, 15–25 cm long; wooden mallet for soft stone |
| Levers | Hardwood poles or iron bars 1.5–2.5 m long; fulcrum blocks |
| Straightedges, square, plumb and level | See Measurement from Scratch |
| Sledge, rollers, ropes | Hardwood sledge; rollers 10–15 cm thick; strong Cordage and Rope |
| Water | For swelling wooden wedges and keeping drill holes clean |
Where to find it
Use Rocks and Minerals to recognise the rock. Good building stone:
- Sandstone and limestone — the easiest to quarry and dress. Look for beds 20–60 cm thick, with few cracks, in cliffs, river cuts and hillsides. Freestone — fine, even sandstone or limestone that can be cut freely in any direction — is the best of all for carving and squaring.
- Slate — for roofs and floors. It splits along its own cleavage into sheets 5–10 mm thick.
- Granite and basalt — very strong and durable, but hard to work. Use loose boulders and naturally jointed blocks first.
- Marble — beautiful, carvable, burns to lime.
Test a stone before opening a quarry. Strike a fresh piece with a hammer: sound stone rings; cracked or rotten stone thuds. Look for clay seams, rusty streaks and crumbling layers — they mark weak stone. Soak a chip in water for a day, then leave it out in a hard frost or let it dry in the sun: stone that crumbles or flakes will not last in a wall. Weigh a dry fist-sized piece, soak it a day and weigh it again: good building stone gains less than about 5% of its weight in water.
Choose the site. Pick a face you can reach from the side, near where the stone is needed or near a downhill track or river. Clear the soil and broken rock (the overburden) off the top until you reach sound stone.
Method 1: Wooden wedges and water
This is the oldest method and needs no metal. It works best in soft, well-bedded stone (sandstone, limestone, slate) where the block is already loose along its bed and joints. It is slow and unreliable in hard granite.
- Mark the line of the split with charcoal. Make it straight, and in a hard stone, follow the rift if you know it.
- Cut slots. With a hard hammerstone, a pick or a stone or copper chisel, cut a row of slots along the line: each slot about 8–12 cm long, 3–5 cm wide and 6–10 cm deep, wider at the top than at the bottom, spaced 15–25 cm apart. In soft limestone this takes perhaps half an hour per slot; in sandstone longer.
- Fit the wedges. Shape dry hardwood wedges to fit each slot snugly, so the wedge bears on the slot's long sides, not on its bottom. A wedge that touches the bottom just lifts itself out.
- Drive them tight with a mallet, all along the row.
- Soak them. Pour water over the wedges and keep them wet — pack wet moss or cloth round them. Dry wood swells by several per cent as it soaks up water and pushes outward with great force. Re-tighten them with the mallet every few hours. A crack may open in hours in soft stone, or not for a day or more.
- Help it along. Tap each wedge in turn along the line. Listen: a high ring means the stone is still holding; a duller thud, and wedges that suddenly go in further, mean the crack is opening.
Tip Wooden wedges work far better when there is already a slight weakness along the line — a bedding plane, a hairline joint, or a deep groove. Historians still argue about how much ancient Egyptian quarrying used water-swelled wood; experiments show it works in soft, layered stone but often fails in hard granite. If it fails, go to Method 2 or 3.
Method 2: Plug and feathers
This is the standard method wherever iron exists, and it works in almost any stone, including granite. The plug is a slim iron wedge; the feathers are two half-round iron strips that line the hole. Their inner faces taper the opposite way to the plug, so plug and feathers together make a bundle with parallel sides that slides into the hole. Driving the plug between the feathers pushes them outward evenly against the sides of the hole.
- Make the tools (see Blacksmithing). For a 2 cm hole: plug 12–15 cm long, a flat wedge about 1 cm thick at the top tapering to 3–4 mm at the tip; feathers 10–12 cm long, rounded on the outside to fit the hole, flat on the inside, and thin at the top, thickening toward the bottom to match the plug's taper, with a little lip bent outward at the top so they hang in the hole. Check the fit: with the plug's tip just between the feathers, the bundle should drop easily into the hole. Harden the plug's tip lightly (Steel); keep the feathers soft enough not to crack.
- Mark the line of the split with charcoal and mark holes along it.
- Hole spacing and depth. In granite: holes 10–15 cm apart and about half as deep as the block is thick (but at least as deep as the feathers are long). In sandstone and limestone, which absorb the force more: holes 15–20 cm apart and two-thirds of the block's thickness deep. Thinner blocks and harder stone need closer holes.
- Drill the holes. Hold the hand drill upright on the mark. Strike its head with a 1–2 kg hammer, then turn the drill an eighth of a turn, strike, turn, strike — the chisel tip chips a round hole. Every few centimetres, pour in a little water and scoop out the paste of rock dust with a stick or a thin spoon. Rough rates: 10–20 cm an hour in granite, two or three times faster in limestone and sandstone. Two people (one holding and turning, one striking a heavier hammer) work faster — but the holder must trust the striker completely.
- Set the plugs and feathers. Drop a pair of feathers into each hole with their flat faces toward each other and in line with the split, so they push outward across the line. Slide a plug between each pair.
- Tap them in turn. Starting at one end, give each plug one or two firm blows, and walk along the row. Then go back and do it again. Do not drive one plug hard while the others are loose — that only cracks the stone around a single hole. Listen for the ring turning to a thud.
- The split. After a few rounds a fine crack appears along the line, runs from hole to hole, and opens. Pull the feathers out, and use levers to open the crack further.
Method 3: Channelling, then wedging the bed
For large blocks of soft limestone or sandstone, Roman and medieval quarry workers cut trenches around the block and then split it free along the bed underneath.
- Mark out the block on the flat top of the bed, with 5–10 cm extra on each side for dressing.
- Cut channels down along the sides of the block that are not already free joints, with picks: channels 8–12 cm wide, deep enough to reach the bedding plane under the block — usually 30–60 cm. The tool leaves typical diagonal "herring-bone" marks.
- Wedge the bed. Drive a row of wedges horizontally into the bedding plane at the bottom of the channel, along the front of the block. The bed is a natural weakness, so it parts easily.
- Lever it out. Push iron bars or hardwood levers into the opened bed and lift. Slide wooden packing under the block as it rises (never put fingers there). Roll it forward onto timbers.
Method 4: Fire splitting
Fire cracks rock because the hot surface expands while the cold rock under it does not. In parts of South India, granite was split into long thin slabs by laying a narrow line of fire along the rock for several hours, then sweeping it away; the heated layer lifted off in a sheet. Fire also helps break up hard stone into rubble for walls and road stone. It is unpredictable for shaped blocks, but it is the basis of fire-setting in Mining and Tunnelling.
Dressing stone
A rough block must be shaped into a dressed stone with flat faces and square corners before it can be laid in a fine wall (called ashlar — walls of squared, dressed stone laid in level courses).
- Pitch off the waste. With a heavy blunt chisel (a pitching tool) or hammerstone held near the edge, knock off big lumps until the block is within 2–3 cm of the size you want on every side.
- Cut the first draft. Along one long edge of the face, cut a straight band about 2–3 cm wide with a flat chisel, checking with a straightedge until light no longer shows under it anywhere.
- Cut the opposite draft. Cut a second draft along the opposite edge. Lay a straight stick (a winding strip) across each draft and sight along the top of the first one to the second. If they are not parallel, the face is in winding (twisted). Cut the high corners down until the two sticks line up exactly.
- Join the drafts with drafts across the two short edges. Now all four edges of the face lie in one flat plane.
- Clear the middle. Remove the stone in the middle with a point chisel, then a claw chisel, then a flat chisel, down to the level of the drafts. Check with the straightedge in every direction.
- Square the next face. Work the adjoining faces the same way, checking each corner with a square. The beds (top and bottom) matter most; the face shown to the world comes last.
- Hold the chisel at an angle. For a point or claw, about 45°; for a flat chisel, nearly flat. Light, frequent blows. A chisel held upright and driven hard bruises the stone below the surface, and it later flakes off.
Most stone should be laid on its natural bed — that is, with its layers horizontal, as they lay in the quarry. Stone stood on edge with its layers vertical tends to peel off in sheets as it weathers. Mark the top of each block with charcoal when you quarry it. Carving mouldings, lettering and figures goes on in Stone Carving.
Moving stone
A block of stone weighs about 2.5 tonnes per cubic metre (sandstone 2.2–2.5, limestone 2.3–2.7, granite 2.7). A block 1 × 0.5 × 0.5 m weighs about 650 kg. Work out the weight before you move anything — the methods and the pulling force needed are in Simple Machines and Moving Goods: Pallet Trucks, Forklifts and Containers:
- Levers and cribbing to lift it a few centimetres at a time, building a criss-cross stack of timbers underneath.
- A sledge on rollers or a wetted track to drag it; downhill whenever you can, with ropes round trees or stakes to hold it back.
- A lewis to lift it with a crane: a dovetail-shaped hole cut in the top of the block (narrow at the top, wider at the bottom), into which three iron pieces are fitted so they lock; a ring through them takes the hook. Or lifting tongs that grip the sides. See Cranes and Lifting.
- Water. A stone on a raft or boat weighs nothing to move sideways; large stones have travelled by river and canal for millennia (Rafts and Canoes, Canals and Locks).
How to tell it worked
- The split. A good split is roughly flat and follows the line of holes, with half-holes showing on both faces.
- Sound stone. A dressed block rings clearly when tapped with a hammer all over; a dull patch means a hidden crack — reject it for lintels, arches and steps.
- Flatness. A straightedge laid on a dressed face in any direction shows no light gap wider than 2–3 mm for rough work, under 1 mm for fine joints.
- Square. Each corner fits a square; the block sits on a flat surface without rocking.
Note Troubleshooting. Crack wanders off the line → holes too far apart or not deep enough, or the line crossed the stone's grain. Drill closer and deeper, and tap wedges evenly. Stone cracks around single holes but does not split → one plug was driven far harder than the rest; tap them all evenly. Wedges jump out → slots too smooth or too V-shaped; make the sides steeper and rougher, or wedge from both ends. Feathers bend or plugs mushroom → iron too soft; reforge and harden the plug tip. Edges break off while dressing → working toward an edge; always chisel from the edge inward, and leave the arrises (corners) until last. Dressed stone flakes after a winter → it was laid on edge or dressed with bruising blows, or it was not frost-proof stone.
Dangers
Danger Falling and rolling stone kills. Never stand under, below or beside a block that is being levered or split, never put a hand or foot under a raised stone — use a stick to push packing in — and never stand downhill of a block on a slope or a sledge. A cubic metre of stone weighs as much as two cars.
Danger Quarry faces collapse. Never undercut a face (dig in at the bottom, leaving an overhang). Work from the top downward in steps (benches) no higher than about 2 m each. After rain or frost, check the face for loose slabs before anyone goes near it, and lever them off from above or the side.
- Flying chips. Drilling, wedging and dressing throw sharp splinters. Protect the eyes (see Rocks and Minerals). Iron tool heads that have mushroomed over shed sharp burrs when hit — grind or forge them clean.
- Hammer blows. In two-person drilling, the holder's hands are inches from a heavy hammer. Practise with light blows, use long handles on the drill, and agree on signals.
- Silica dust. Dry drilling and dressing sandstone and granite fill the air with dust that causes silicosis. Keep holes and surfaces wet, work outdoors and upwind, and cover your nose and mouth with a damp cloth.
- Strains and crushed fingers. Lift with your legs and with enough people; use levers rather than backs.
What this unlocks
Dressed blocks make Stone Masonry, Foundations and Floors, Arches, Vaults and Domes, bridges (Roads and Bridges) and lined Wells and Cisterns. Quarried limestone feeds Lime kilns and Portland Cement works. Quarrying skills lead underground into Mining and Tunnelling. Good sandstone becomes millstones for The Watermills and grindstones (Abrasives and Grinding Stones).
How it was first done
Quarrying began with flint: Neolithic people dug pits and shafts into chalk for good flint by about 4000 BC (see Mining and Tunnelling). Egyptian builders quarried soft limestone with copper chisels and wooden mallets from about 2700 BC, and cut hard granite at Aswan by pounding it with balls of even harder dolerite — the unfinished obelisk there, about 42 m long and perhaps 1,100 tonnes, still lies in the trench where they abandoned it when it cracked. Romans quarried limestone and marble across their empire with picks, channels and iron wedges; at Baalbek in Lebanon, blocks weighing around 800–1,000 tonnes were cut and some were moved into a temple platform. The Inca of Peru dressed hard andesite and granite with hammerstones into blocks that fit without mortar. Splitting with plugs and feathers in round drilled holes is probably younger — exactly when it began is uncertain — but by the 18th and 19th centuries it was the quarry worker's standard method, and it is still used by hand today alongside power drills and diamond saws.
Source: content/entries/earth/quarrying-stone.md