◆ Rebuild

Part 3 · Metals

Aluminium

The most common metal in the Earth's crust, and once more precious than silver because no fire can free it. Refine red bauxite into pure white alumina, dissolve it in molten cryolite, and pull the metal out with a heavy electric current — the Hall–Héroult process.

Difficulty
●●●●●
Time
Weeks to prepare alumina and cryolite; days to start a cell; then continuous production for months
Steps from zero
28 prerequisites →

You need first

ElectrolysisThe Electric Arc Furnace

This unlocks

Anodising Aluminium and Titanium
The full path from nothing — 28 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Bricks
  14. Fermentation
  15. The Wheel and Axle
  16. Firebrick and Refractories
  17. Bellows
  18. Gears
  19. Copper Smelting
  20. Iron (the Bloomery)
  21. The Waterwheel
  22. Blacksmithing
  23. The Battery
  24. Magnets
  25. Electrolysis
  26. Copper Wire
  27. The Generator
  28. The Electric Arc Furnace
  29. Aluminium

Do them roughly in this order. See it on the tech tree →

Why it matters

Aluminium is a third of the weight of steel or copper, does not rust, conducts electricity and heat very well, reflects light like a mirror, and melts at only 660 °C, so it casts easily in sand. It is the metal of:

But aluminium is hard. It is not a metal you can smelt in a furnace. It needs a very large, steady supply of direct-current electricity, very pure raw materials, and a special molten salt. In 1855 a bar of it was shown beside the crown jewels in Paris. In 1886 two young men found the method in this chapter, and within a few decades aluminium became one of the cheapest metals of all. Do this only when you have Electrolysis working and many kilowatts of power — a hydroelectric plant (Water Turbines and Hydroelectric Power) is ideal.

How it works

Aluminium is everywhere — in every clay, feldspar and mica — but it is joined to oxygen more tightly than almost any other metal. Charcoal cannot pull the oxygen away in any ordinary furnace. In water, electrolysis gives hydrogen instead of aluminium. And pure aluminium oxide, alumina, melts only at 2,050 °C.

The Hall–Héroult trick: molten cryolite (sodium aluminium fluoride) melts at about 1,000 °C, and alumina dissolves in it as sugar dissolves in tea. Pass a heavy direct current through this molten bath between carbon electrodes:

  • At the cathode (negative, the carbon floor of the pot), aluminium collects as liquid metal. It is denser than the bath and sinks into a shining pool.
  • At the anode (positive, carbon blocks dipping in from above), the oxygen combines with the carbon and bubbles off as carbon dioxide. The anodes are slowly eaten away.
  • The cryolite itself is not used up. You feed in alumina, and take out aluminium.

The current also keeps the bath hot: a big cell produces its own heat from the resistance of the bath and needs no fire.

The numbers

For each kilogram of aluminium
Alumina about 2 kg (from 4–5 kg of good bauxite)
Carbon anode consumed 0.45–0.6 kg
Electric charge 2,980 ampere-hours in theory (1 A for 1 hour gives 0.34 g) — about 3,500 in practice
Voltage per cell 4–6 V
Energy 13–15 kWh in a modern plant; 20–30 kWh or more in a small home-built cell
Cryolite used only to start; small losses each week

So a single cell running on 1,000 A at 5 V (5 kW) gives about 6–8 kg of aluminium a day. Cells are connected in series (the cathode of one to the anode of the next) so a 100 V generator can drive about 20 of them at once.

What you need

Item Notes
Bauxite, or clay The ore. See below.
Caustic soda (or soda ash and lime) To dissolve alumina out of bauxite. See Lye and Potash and Soda Ash and Baking Soda.
Cryolite Natural, or made from fluorite. For a 1,000 A cell, 150–250 kg of bath.
Carbon Coke and pitch for anodes and the pot lining. See The Electric Arc Furnace for making carbon electrodes.
Iron pot Riveted iron plate, for a 1,000 A cell about 1 m × 0.6 m and 0.5 m deep outside.
Firebrick and alumina powder To insulate the pot. See Firebrick and Refractories.
DC power A low-voltage dynamo (see The Generator) giving hundreds to thousands of amperes, plus heavy copper or aluminium bus bars.
Tools Iron bars for breaking crust, iron ladle, ingot moulds, a lamp wired across the cell

Where to find it

  • Bauxite is the weathered remains of rock in hot, wet climates — the tropics, or places that were tropical long ago (it was named after Les Baux in southern France). Look for red-brown, pink, cream or mottled earthy rock, often made of little rounded pea-sized grains (pisoliths), in thick layers under red tropical soils on plateaus. It looks like clay but does not become sticky and plastic when wet, and it is light for a rock of its colour. A good test: boil a powdered sample in strong lye — a good bauxite dissolves largely, leaving a red-brown sludge.
  • Clay is a poorer but universal source: about 20–40% alumina, mixed with silica that is hard to separate. See Finding and Preparing Clay.
  • Fluorite (calcium fluoride) is found in veins, often with Lead ore (galena), quartz and calcite, especially in limestone country. It forms cubes or breaks into neat eight-sided pieces; glassy; purple, green, yellow, blue or colourless, often banded; soft enough to scratch with a steel knife, but it scratches copper. Many pieces glow faintly when heated in the dark.
  • Cryolite occurs in quantity at only one place on Earth — Ivittuut in south-west Greenland, now mined out. It is white, glassy, and almost invisible in water. In practice, you will have to make it.

Step 1: Pure alumina from bauxite

The alumina must be pure white. Every bit of iron or silica in it ends up in your aluminium.

bauxite soda ash clear CO₂ 1. Grind and mix bauxite with soda ash(and limestone ifthere is much silica) 2. Roast 1,000–1,100 °C,3–4 hours: aluminajoins the soda 3. Leach hot water dissolves it;red mud (iron) settles;pour off the clear liquid 4. Precipitate bubble CO₂ through:white aluminiumhydroxide settles 5. Calcine 1,100–1,200 °C:pure white alumina,ready for the cell
Fig. 1 From red bauxite to white alumina. The aluminium is dissolved out as sodium aluminate, the red mud of iron oxide is settled away, and pure aluminium hydroxide is grown from the clear liquid and roasted to alumina.

Method A: The sinter route (no pressure vessel)

This is the older route of Henri Sainte-Claire Deville and Louis Le Chatelier.

  1. Grind dried bauxite to a fine powder. Mix it with powdered soda ash, about 1 part to every 1–1.5 parts of bauxite by weight, and, if your bauxite contains much silica, some powdered limestone (about twice the weight of the silica) to lock the silica up as an insoluble calcium compound.
  2. Roast the mixture in a reverberatory furnace or kiln at a bright orange heat (about 1,000–1,100 °C) for 3–4 hours, stirring now and then. The alumina combines with the soda into sodium aluminate, which dissolves in water.
  3. Leach. Crush the cooled mass and soak it in hot water, stirring, then let it settle. Pour off the clear, slightly yellow liquid. Leach the red residue twice more and combine the liquids.
  4. Precipitate. Bubble carbon dioxide — the clean gas from a Lime kiln or from burning charcoal, washed through water — through the liquid, stirring, for several hours. White, gelatinous aluminium hydroxide settles out. Stop while the liquid is still slightly alkaline (it still feels soapy), or silica comes down too.
  5. Wash the white precipitate several times in clean water, and dry it.
  6. Calcine. Roast it in a clean clay or alumina container at 1,100–1,200 °C (yellow-white) for several hours. It loses about a third of its weight as water and becomes alumina: a fine, white, gritty powder.
  7. Recover the soda. Boil down the remaining liquid: it contains soda ash, which you can use again.

Method B: The Bayer process (with a pressure boiler)

This is how almost all alumina is made today, and the largest example of Leaching, Solvent Extraction and Electrowinning — winning a metal compound by dissolving it out of ore. Digest finely crushed bauxite in strong caustic soda solution (see Lye and Potash) in a closed iron boiler at 140–150 °C (about 3–4 times atmospheric pressure) for an hour or two. Let the red mud settle, filter the clear liquid, cool it to about 60 °C, and stir in a few handfuls of fine aluminium hydroxide from a previous batch as seed. Over 1–3 days of slow stirring, the aluminium hydroxide crystallises out onto the seed. Filter it, wash it, and calcine it as above. The caustic liquid goes back to dissolve more bauxite. The boiler must be built and tested like a The Steam Engine boiler.

From clay

Without bauxite, dissolve the alumina out of clean white clay with hot dilute Sulfuric Acid, then add potash (Lye and Potash) to crystallise alum. Recrystallise the alum two or three times to purify it; dissolve it, precipitate aluminium hydroxide with soda ash solution, wash and calcine. It is slow and expensive, but clay is everywhere. The full method is in Alum and Alumina.

Step 2: Cryolite

Synthetic cryolite is made from hydrofluoric acid, which comes from fluorite and sulfuric acid. This is the most dangerous step in this chapter: read the dangers first, and do it only with experienced chemists, in the open air.

In outline: fluorite and Sulfuric Acid give hydrogen fluoride; dissolved in water it is hydrofluoric acid; aluminium hydroxide from Step 1 and then Soda Ash and Baking Soda turn it into cryolite, which comes down as a fine white powder. Because hydrofluoric acid can kill through a splash that does not even hurt at first, this book gives it only in outline — see Fluorspar and Fluorine Compounds for why, and treat this as work for a trained chemist with a proper fume plant and calcium gluconate gel at hand.

Because the bath is not used up, you make cryolite once. A small cell's bath can run for years with small top-ups. Adding about 5–10% aluminium fluoride and 4–6% fluorite to the cryolite lowers its melting point to about 950 °C, saving power.

Step 3: The cell

Bus bar (+)from the generator Carbon anodesburn away; lower them Crustfrozen bath + alumina Molten bathcryolite + 3–5% alumina,960–1,000 °C, orange Liquid aluminium Carbon liningthe cathode (−) Insulation in an iron shell Signal lamplights at 20–40 V:add alumina Gap 4–5 cmanode to metal to (−) of generator CO₂ escapes through the crust
Fig. 2 The Hall–Héroult cell. Carbon anodes hang into the molten cryolite bath; aluminium collects on the carbon floor, which is the cathode. A frozen crust of bath and alumina on top keeps the heat in.

Building it

  1. The pot. An iron box, lined inside with 15–20 cm of firebrick and alumina powder for insulation on the sides and bottom.
  2. The carbon lining. Inside the insulation, ram a lining of carbon paste (the same coke-and-pitch paste as for electrodes) 10–15 cm thick on the bottom and walls, leaving a cavity about 25–30 cm deep. Bed several iron collector bars in the bottom carbon, passing out through the side of the pot to the negative bus bar. Bake the lining slowly with a coke fire inside, as for electrodes.
  3. The anodes. Baked carbon blocks (see The Electric Arc Furnace), each with an iron rod cemented into a hole in the top. Hang them from a copper or aluminium bus bar on a frame, so you can raise and lower each anode. Give them about 1 A for every 1–1.5 cm² of underside: a 1,000 A cell needs about 1,000–1,500 cm² of anode face — for example two blocks each 25 × 25 cm.

Starting it

  1. Preheat. Fill the cavity with coke and lower the anodes onto it. Turn on the current: the coke heats up like a stove element. Over 1–2 days bring the lining up to a bright red heat.
  2. Melt the bath. Rake out the coke and shovel in crushed cryolite. Raise the anodes a little as it melts so an arc does not form. When you have a 10–20 cm deep molten bath, glowing orange-yellow (about 960–1,000 °C), add alumina: about 3–5% of the bath weight.
  3. Set the gap. Lower the anodes so they dip about 5 cm into the bath and their lower faces are about 4–5 cm above the cathode floor (later, above the aluminium pool). The cell voltage should settle at about 5–6 V.

Running it

  1. Feed alumina every half hour to hour: break the crust with an iron bar and push in fresh alumina, a little at a time.
  2. Watch for the "anode effect". When the alumina runs low, a film of gas covers the anodes and the voltage across the cell suddenly jumps to 20–40 V. Wire an ordinary lamp across the cell: it stays dark at 5 V and lights up at 30 V. When it lights, break the crust, add alumina and stir with a green wooden pole; the voltage drops back at once.
  3. Lower the anodes gradually as they burn away; replace each one when it is two-thirds consumed.
  4. Keep the crust. A frozen layer of bath and alumina on top keeps the heat in. Pile alumina on it — this also warms the alumina before it goes in.
  5. Tap the metal every 1–3 days. Ladle or siphon aluminium from the pool at the bottom, leaving a few centimetres behind to protect the floor. Pour it into iron moulds.

A cell with a well-baked lining can run continuously for months. Do not let it freeze: a frozen cell usually has to be dug out and relined.

Tip Start small. Charles Martin Hall's first success in 1886 was a few small globules of aluminium from a crucible lined with carbon, heated in a furnace and fed by a bank of home-made batteries. Do the same before building a full cell: a carbon crucible holding 1–2 kg of cryolite, heated from outside in a coke furnace, a carbon rod as anode, and 20–50 A from batteries or a dynamo. After a few hours you should find shiny beads on the bottom.

Melting and using aluminium

  • Remelt in an iron or clay crucible at 700–750 °C — barely a dull red glow in a dark room. Skim the grey dross off the top. Pour into dry, warmed sand moulds (see Metal Casting).
  • Casting alloy: add 7–12% silicon (from The Electric Arc Furnace) — it flows better and shrinks less.
  • Strong alloy (duralumin): 4% copper, 0.5% magnesium, 0.5% manganese. After quenching from 500 °C in water, it hardens by itself over 4–5 days at room temperature.
  • Rolling and drawing: pure aluminium rolls easily into sheet and foil (Sheet Metal and Rolling) and draws into wire (see Copper Wire and Iron and Brass Wire).
  • Joining: aluminium is hard to solder and weld because of its tough oxide skin; rivet it, or see Welding.
  • Protecting and colouring: the thin natural oxide skin can be grown thick, hard and dyed by Anodising Aluminium and Titanium.
  • Recycling: remelting scrap aluminium takes about 5% of the energy of making new. Never throw it away.

How to tell it worked

  • Weight. An aluminium bar weighs about a third of an iron bar of the same size.
  • Look. Silvery-white, bright when cut, dulling to a soft grey but never rusting.
  • Magnet. Not attracted.
  • Lye test. A small chip dropped into strong lye fizzes vigorously and slowly dissolves, giving off hydrogen. Iron does not (zinc also fizzes, so use this with the weight and magnet tests).
  • Softness. Pure aluminium is soft: it bends easily, and a steel knife cuts shavings from it.

Note Troubleshooting. Metal grey, brittle and heavy → iron or silicon from impure alumina, or iron tools left in the bath. Purify the alumina; keep iron out of the bath. Anode effects every few minutes → feeding too little alumina, or too much at once so it sinks unmelted as "sludge". Feed little and often. Bath freezes around the edges and the cell cools → too little current for the size, or poor insulation. Insulate better; lower the anodes slightly to raise the current; at small sizes, heat from outside. No metal after hours → anode–cathode gap too small (metal burns back at the anode), or bath too hot. Widen the gap to 4–5 cm; keep the bath orange, not white. Carbon lining cracks and bath leaks into the insulation → lining not baked slowly enough. Bake for days, not hours.

Dangers

Danger Hydrofluoric acid and fluoride fumes. Hydrogen fluoride and hydrofluoric acid are among the most dangerous chemicals in this book. A splash on the skin may not hurt for hours while it passes through the skin into the blood and bone, and a burn from strong acid covering not much more than the palms of both hands can kill by poisoning the heart. Make it only in the open air, standing upwind, with thick rubber or waxed leather gloves, an apron and a face shield, and with plenty of water and chalk or lime paste ready to wash and cover any splash. Never use glass or glazed vessels for it.

Danger Molten bath and water. Cryolite at 1,000 °C and liquid aluminium explode violently on contact with water or damp tools, damp alumina or wet moulds. Dry and preheat everything that goes into the cell. Molten aluminium hitting a damp concrete or stone floor can blast it apart.

Danger Electricity. One cell is only 5 V, but a line of twenty is 100 V DC and can kill. The heavy bus bars can also burn and weld anything metal that bridges them. Never touch two cells at once; stand on dry wood; keep rings and tools away from bus bars.

  • Fluoride fumes from the cell slowly damage the bones and teeth of workers, and of animals and plants downwind. Keep the cell crusted over, ventilate well, and site the plant away from grazing land.
  • Carbon monoxide and dioxide come from the anodes. Work in a high, airy building.
  • Invisible heat. Aluminium at 700 °C barely glows in daylight. Treat every pot and ingot as hot.
  • Lye used in refining bauxite blinds. Wear eye protection — see Lye and Potash.
  • Fine aluminium powder can burn fiercely and its dust can explode. Keep grinding dust out of the air and away from flames.

What this unlocks

Aluminium wire for long Power Lines and Distribution lines; light engines for the The Motor Vehicle and Gliders and Aeroplanes; mirrors for the The Telescope; cookware and foil for Canning and Bottling and Preserving Food; and alumina itself as a high-grade refractory (Firebrick and Refractories) and an abrasive (Abrasives and Grinding Stones). Aluminium powder burned with iron oxide (the thermite reaction) gives liquid iron for welding railway rails — see Welding.

How it was first done

Hans Christian Ørsted in Denmark made the first impure aluminium in 1825, reducing aluminium chloride with potassium amalgam. Friedrich Wöhler in Germany made it as powder in 1827 and as small beads in 1845. In 1854 Henri Sainte-Claire Deville in France found a way to make it with sodium, and Emperor Napoleon III supported the work; aluminium then cost about as much as silver. In 1884 a cap of aluminium weighing about 2.8 kg was set on top of the Washington Monument as a precious curiosity.

In February 1886, Charles Martin Hall, a 22-year-old graduate of Oberlin College in Ohio, working in a woodshed with help from his sister Julia, ran a current from home-made batteries through alumina dissolved in molten cryolite and found buttons of aluminium. Paul Héroult in France, also 22, discovered the same process independently that same year. Karl Josef Bayer, an Austrian chemist working in Russia, patented his alumina process in 1888. Hall's company (later Alcoa) began production at Pittsburgh in 1888, and aluminium's price fell steeply as large hydroelectric plants, starting at Niagara Falls in the 1890s, supplied the power.