Diamond is the hardest thing there is, and the ugly, flawed stones no jeweller wants — bort and black carbonado — are the most useful. How to find and recover them, crush them to graded powder, and set them as the wheel dressers, saws, drills and wire-drawing dies that shape every other hard material; how to make the next-hardest abrasives, silicon carbide and boron carbide, in the arc furnace; and, in outline, how diamond itself is made from graphite under enormous pressure.

Difficulty
●●●●●
Time
Days to weeks to find and recover stones; an afternoon to crush and grade powder; a day to set a dresser or charge a saw; weeks for a fine wire die by hand
Steps from zero
25 prerequisites →

You need first

Abrasives and Grinding StonesThe Electric Arc Furnace

This unlocks

—
The full path from nothing — 25 steps before this one
  1. Stone Tools
  2. Fire
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Abrasives and Grinding Stones
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Bricks
  14. The Wheel and Axle
  15. Firebrick and Refractories
  16. Bellows
  17. Gears
  18. Iron (the Bloomery)
  19. Copper Smelting
  20. The Waterwheel
  21. Blacksmithing
  22. Magnets
  23. Copper Wire
  24. The Generator
  25. The Electric Arc Furnace
  26. Industrial Diamond and Hard Abrasives

Do them roughly in this order. See it on the tech tree →

Why it matters

Every abrasive cuts only what is softer than itself. Sand cuts bronze, emery cuts steel, corundum cuts hardened steel and quartz (Abrasives and Grinding Stones, Synthetic Gems). But to true a corundum grinding wheel, to saw granite quickly, to bore a rock tunnel, to drill a ruby or to draw tungsten wire finer than a hair, you need something harder still. There are only a few such materials, and diamond stands far above them all.

Industrial diamond does jobs that nothing else can:

Silicon carbide and boron carbide, made in the The Electric Arc Furnace, are nearly as hard and can be made by the tonne. They take over most grinding work; diamond is kept for the jobs where only diamond will do.

How it works

Hardness. On Mohs' scale — a ranking in which each mineral scratches those below it — quartz is 7, topaz 8, corundum 9 and diamond 10. But the steps are uneven. Diamond is about four times as hard as corundum when measured by how deep a point sinks in. Between them stand silicon carbide (about 9.5) and boron carbide (a little harder).

Why diamond is so hard. It is pure carbon, each atom bonded tightly to four neighbours in a rigid three-dimensional frame. Graphite is the same carbon arranged in slippery sheets — which is why it is soft. At ordinary pressures graphite is the stable form; diamond forms only at enormous pressure, deep in the Earth (or in a press), and survives on the surface because changing back is so slow.

Diamond's weaknesses decide how you use it:

  • It cleaves: a sharp blow along certain planes splits it like slate. Set it so the load presses it into its seat, never so it is levered or knocked.
  • It burns. Heated in air above about 700 °C it slowly turns to carbon dioxide, and it begins turning to graphite at higher heats. Never let it get red-hot in air. Run it wet.
  • It dissolves in hot iron. Cutting steel at speed, diamond wears away quickly because carbon dissolves into the hot iron. Use diamond for stone, glass, ceramics, carbide, non-ferrous metals and wheel dressing — and use carbide, corundum or cubic boron nitride (below) for steel.

What you need

Item Use See
Diamond-bearing gravel or crushed kimberlite Source of stones Below
Sieves, pans or a jig, and a grease table Recovery Finding and Identifying Ores
A hardened steel diamond mortar Crushing bort Below, Steel
Olive oil or a light vegetable oil, glass jars Grading powder Oils and Pressing
Mild steel or brass rod, silver brazing alloy, borax Setting dressers and tools Soldering and Brazing
Soft copper or iron discs, bronze or cobalt powder Saws Copper Smelting, Nickel and Cobalt
An arc furnace, sand, coke, sawdust, salt; borax and carbon Silicon carbide and boron carbide The Electric Arc Furnace, Borax and Boric Acid

Where to find it

Diamond crystals are usually octahedra (two four-sided pyramids base to base) with slightly curved, rounded faces, often bearing tiny triangular pits; also cubes, flattened triangles (macles) and broken pieces. Clear, yellowish, brown or grey, with a greasy-looking, brilliant (adamantine) shine. They scratch everything, including corundum, and nothing scratches them but another diamond. They weigh about 3.5 times their volume of water — heavier than quartz, lighter than garnet. Water will not wet a diamond; it beads up and runs off, while grease clings to it. A diamond touched to the lip feels distinctly cold, because it carries heat away faster than any other material.

Industrial grades.

  • Bort (or boart) — badly formed, flawed, cloudy or broken diamonds, unfit for gems. Most diamonds dug up are bort. It is crushed to powder or used as small stones.
  • Carbonado — black, porous, tough lumps made of countless tiny diamond crystals grown together, found in Brazil and the Central African Republic. Because the crystals point every way, it does not cleave, so it was prized for rock drills.
  • Ballas — round balls of radiating diamond crystals; very tough.

Where diamonds occur. They come up from more than 150 km deep in narrow carrot-shaped volcanic pipes of kimberlite, found only in the ancient, stable cores of continents: southern and central Africa, Siberia, northern Canada, Brazil, India, western Australia. Weathered kimberlite at the surface is soft yellow ground, then blue ground below. More often, rivers and seas have worn the pipes away and carried the diamonds into gravels: old river terraces, the inside bends of streams below such country, and beach gravels. India's ancient diamonds, Brazil's, and those of the West African rivers and the Namibian coast were all dug from gravels.

Signs of kimberlite in stream sand: grains of purple-red pyrope garnet, bright emerald-green chrome diopside, and black glassy ilmenite. Trace these "indicator minerals" upstream to their source.

Recovering diamonds

  1. Wash and screen gravel or crushed yellow ground through sieves, keeping the 1–25 mm part.
  2. Concentrate it by panning or jigging (Finding and Identifying Ores, Mining and Tunnelling). Diamond is moderately heavy, so it goes to the bottom with garnet and iron minerals while light sand washes away. Do not throw away the heavy part unless you have searched it.
  3. Grease table. Build a sloping table about 1 m long and 50 cm wide, at about 10–15°, and smear it with a layer of thick grease 3–5 mm deep — petroleum jelly (Petroleum and Refining), or tallow softened with a little oil. Wash the wet concentrate down it in a steady stream of water. The wet minerals slide over and off; diamonds stick in the grease. Scrape the grease off into a wire basket and boil it in water: the grease melts away and the stones remain.
  4. Check by hand on a clean white tray. Test any doubtful stone by scratching a piece of corundum or a ruby (Synthetic Gems) with it.
Wet concentrate washed on with water Diamonds stick water cannot wet them Wet minerals slide off garnet, ilmenite, sand Grease 3–5 mm deep table about 1 m long, 10–15° slope Tailings tub
Fig. 1 Diamonds stick to grease. Wet concentrate washed down a greased table runs off into the tailings tub; diamonds, which water cannot wet, stick in the grease.

Diamond powder

  1. Crush. Use a diamond mortar: a block of hardened tool steel with a hole 15–20 mm across and 30 mm deep, and a close-fitting hardened steel pestle. Drop in a few small bort stones, put in the pestle and strike it with a hammer, then turn and strike again. Diamond is hard but brittle and shatters into sharp grains. The mortar wears a little and adds iron.
  2. Clean. Boil the powder in Hydrochloric Acid to dissolve the iron from the mortar, then wash it in water many times. Dry it.
  3. Grade by settling, as in Abrasives and Grinding Stones, but in olive oil rather than water: oil settles fine diamond more slowly and evenly, and keeps it from clumping. Stir the powder into a tall jar of oil and pour off the cloudy oil after 1 minute, 10 minutes, 1 hour, 12 hours and several days in turn; each settling is one grade. Coarse grades (about 0.05–0.1 mm) charge saws and drills; medium (0.01–0.04 mm) for laps; the finest (a few thousandths of a millimetre) for polishing.
  4. Paste. Mix each grade with tallow or petroleum jelly and a few drops of oil, and keep it in a labelled pot. A matchhead of paste does a great deal of work.

Diamond dresser

The tool that trues and sharpens grinding wheels (Precision Grinding): a single diamond point set in the end of a steel rod.

Dresser Charged disc saw Segment saw Diamond ¼–1 carat Peened rim or silver-brazed Shank 10–12 mm steel or brass; stone ⅔ buried, point out Hardened roller closes the nicks Nicks 1–2 mm apart soft copper or iron disc, 15–20 cm, 0.5–0.8 mm thick; diamond powder in oil Segments diamond in bronze Gullet steel disc 30–100 cm; segments brazed on; run wet at 30–40 m/s
Fig. 2 Three diamond tools. A dresser: one stone set in the end of a steel shank. A charged saw: diamond powder hammered into nicks in a soft copper rim. A segment saw: sintered bronze segments full of diamond grit, brazed to a steel disc.
  1. Choose the stone. A whole, crack-free bort crystal of 0.05–0.2 g (¼ to 1 carat; 1 carat = 0.2 g), with a natural sharp point. Bigger wheels need bigger stones.
  2. Prepare the shank: mild steel or brass rod 10–12 mm across and 120–150 mm long. Drill a hole in the end a little larger than the stone, deep enough to hold about two-thirds of it.
  3. Set it by one of two ways:
    • Peen (cold): seat the stone, point out, in the hole on a bed of copper filings; tap the rim of the hole down over the stone all round with a small punch and light hammer, a little at a time, until it is gripped firmly. Like setting a jewel (Jewellery, Beads and Medals).
    • Braze: pack the stone into the hole with fragments of silver brazing alloy and plenty of borax, and heat the end quickly to a bright red — no hotter, no longer — until the alloy flows round the stone (Soldering and Brazing). The borax shields the diamond from the air. Cool slowly.
  4. Use it at 10–15°, trailing the direction of the wheel, slightly below centre, flooded with water, taking 0.01–0.03 mm per pass. Turn the shank an eighth of a turn every few dressings, so the stone wears to a cone instead of a flat. When the point is gone, unset the stone and reset it with a fresh point outward.
  5. Cluster dressers for rough work hold several bort chips in a lump of sintered bronze, made as for saw segments below.

Diamond saw

The charged disc — the oldest and simplest, for gems, glass and small stone.

  1. Cut a disc of soft copper or soft iron 15–20 cm across and 0.5–0.8 mm thick, true it on a lathe, and fit it on a spindle with flanges at least a third of its diameter.
  2. With a knife-edged chisel, cut small nicks into the rim every 1–2 mm, about 1 mm deep.
  3. Fill the nicks with coarse diamond powder in oil — about 0.1–0.2 g (half a carat to a carat) for a 15 cm disc.
  4. Roll a smooth hardened steel roller round the rim with firm pressure, closing the nicks over the grains and pressing more into the soft metal.
  5. Run it at 2,000–3,000 turns a minute with a drip of water or paraffin oil, feeding the work slowly. It cuts agate or glass many times faster than a loose-grit saw (Gem Cutting and Lapidary). Recharge when it slows.

The segment saw — for building stone, concrete and tile.

  1. Mix coarse diamond grit (0.3–0.6 mm) at about 3–5% by volume with fine bronze powder (8 parts copper to 2 of tin, Bronze) or cobalt powder.
  2. Press it into a graphite mould to make segments about 40 × 10 × 4 mm, and sinter them at 750–900 °C under pressure, in hydrogen or in the graphite mould heated by its own current, so air never reaches the diamonds.
  3. Braze the segments with silver alloy round the rim of a steel disc 30–100 cm across, with a slot (gullet) between each to clear the slurry.
  4. Run it with plenty of water at a rim speed of 30–40 metres a second (for a 40 cm blade, about 1,500–2,000 turns a minute). As the bronze wears, fresh diamonds come to the surface; a blade that glazes (stops cutting and polishes) needs to be run through a soft sandstone to open it.

Wire saws for quarries thread small sleeves of the same sintered diamond material, every 25–30 mm, on a steel wire rope (Wire Rope and Cable) that runs as a loop round the block of stone.

Diamond core drill

A steel tube with a crown of diamonds set round its end cuts an annular groove and brings up a solid core of rock — the way to sample ore bodies and foundations deep below ground (Mining and Tunnelling). Set small carbonado or bort stones in holes round a soft steel crown ring by peening or in a sintered bronze crown, half of them projecting on the outside edge and half on the inside, so the hole is larger than the tube and the core smaller. Turn it at 100–600 turns a minute with water pumped down the inside, and lift the core out in a tube with a spring catch at the bottom.

Diamond die

Steel or brass casing Diamond Wire in Wire out, smaller pull Bell (entry) about 60° Reduction cone 12–18° included Bearing ½ wire diameter long Back relief
Fig. 3 A diamond wire-drawing die in section. The wire enters through the wide bell, is squeezed down in the reduction cone, takes its final size in the short straight bearing, and leaves through the back relief. The stone is held in a steel or brass casing.

For wire below about 1 mm, the diamond die is the finest tool there is. It is slow, patient work.

  1. Select a clear, crack-free stone of 0.02–0.2 g (0.1–1 carat), bigger for bigger wire.
  2. Grind two flat windows on opposite sides on a lap charged with coarse diamond paste, so you can see into the stone and it sits flat.
  3. Drill a pilot hole. Mount the stone firmly. Twirl a fine steel needle, charged with diamond powder in oil, back and forth in a small bow drill or a slowly rotating spindle, pressing gently. Drill from both sides until the holes meet. By hand this takes days to weeks; be patient, and never let the stone heat.
  4. Shape the profile with pointed steel needles of the right angle, charged with ever finer powder:
    • Bell (entry): a wide funnel, about 60° included angle, guiding the wire and its lubricant in.
    • Reduction cone: about 12–18° included angle for copper and brass, a little narrower for hard metals. Here the wire is squeezed down.
    • Bearing: a short straight cylinder, about half the wire diameter long, that sets the final size.
    • Back relief: a short cone opening out behind, so the bearing's edge does not scrape the wire.
  5. Polish the bore by pulling a fine wire charged with the finest paste back and forth through it, until a wire drawn through comes out mirror-bright.
  6. Mount the stone in a steel or brass casing about 25 mm across: seat it in a recess and cast brass or press a ring of soft metal round it, or sinter metal powder round it.
  7. Size it by drawing a test wire and weighing a 200 mm length (Tungsten and Filament Wire).

A set of dies, each about 10–20% smaller in area than the last, goes on a drawing machine (Iron and Brass Wire). A diamond die draws hundreds of times more wire than a steel plate before it grows oversize; then it is opened to the next larger size and used again.

Silicon carbide and boron carbide

Silicon carbide (carborundum) is made in the The Electric Arc Furnace from quartz sand and coke, with sawdust to keep the charge open and salt to carry off iron; the recipe is in Precision Grinding. After the run, break the furnace open: round the core lies a shell of glittering crystals, green where purest, black where less pure. Pick the best, crush them in rolls or under a hammer, boil the grit in dilute acid and then in Lye and Potash to clean it, and grade it by sieving and settling. Green grit grinds carbide tools, glass, stone and cast iron; black grit grinds castings and stone. Silicon carbide also makes refractory shelves and rods that glow as furnace heating elements (Electric Kilns and Furnaces, Firebrick and Refractories).

Boron carbide is harder still and very light — about 2.5 times the weight of water. Make boric oxide by heating boric acid until it melts to a glass (Borax and Boric Acid); grind it with carbon (coke or charcoal), about 6–7 parts carbon to 10 of boric oxide by weight, and heat it in the arc furnace to about 2,400 °C. It comes out as black, shining crystals. Crushed and graded, it is the best loose grit for lapping carbide tools, rubies and other gems when diamond is short. Pressed and sintered, it makes sandblast nozzles that outlast steel many times over, and its boron soaks up neutrons, so it goes into the control rods of reactors (Nuclear Energy (Overview)).

Synthetic diamond, in outline

Diamond can be made from graphite, but only with industry behind you.

  • High pressure and heat. Graphite is packed with a metal solvent — iron, nickel or cobalt — inside a cell of soft stone such as pyrophyllite, which flows to seal it and passes on the pressure. The cell is squeezed between pistons of tungsten carbide (Tungsten and Filament Wire), backed by steel rings, to about 55,000 atmospheres (about 560 kg on every square millimetre), and heated to 1,300–1,600 °C by a current through a graphite tube inside it. The graphite dissolves in the molten metal and crystallises out as diamond, in minutes. It takes a hydraulic press of hundreds to thousands of tonnes (Hydraulic Presses and Rams). The product is small yellow crystals, 0.1–1 mm — exactly the grit grinding wheels and saws need.
  • From gas. At low pressure, a mixture of about 1% methane in hydrogen (Natural Gas and Helium, Hydrogen, Oxygen and Gases) is broken up by a white-hot tungsten wire or a microwave discharge, and diamond grows slowly as a film on a surface held at 700–1,000 °C.
  • Cubic boron nitride is made in the same presses from boron nitride. It is almost as hard as diamond and does not dissolve in hot iron, so it is the wheel and tool for grinding hardened steel.

Neither is a first-generation project. Use natural bort until your industry can build carbide anvils and giant presses.

How to tell it worked

  • Diamond: scratches corundum easily; water beads on it; feels cold to the lip; sticks to grease.
  • Powder: each grade looks even under a magnifier; a pinch of the coarsest scratches a sapphire.
  • Dresser: leaves a wheel cutting cool and freely, with a fine, even surface; the stone does not move in its seat when pressed with a thumbnail.
  • Saw: cuts steadily with light pressure and no burning smell; the kerf is straight.
  • Die: wire comes out bright, round, of constant weight per length, without scratches or a "fin".
  • Silicon carbide and boron carbide: scratch hardened steel and quartz easily; boron carbide grit scratches silicon carbide.

Note Troubleshooting. Stone falls out of the dresser → seat too shallow or peening uneven; reset it deeper. Diamond turned milky or black on the surface → overheated in brazing or used dry. Heat less, braze faster under more borax, always run wet. Charged saw stops cutting → diamond worn or stripped; recharge. If it wanders, the disc is warped: true it on the lathe. Segment blade glazes → bond too hard for the stone, or too little water. Dress it in sandstone; next time use a softer bond (less tin, more copper), since tin is what hardens bronze. Die draws scratched wire → a chip or grain in the bore; repolish. Diamond tool wears fast on steel → diamond and hot iron do not mix. Use carbide or corundum.

Dangers

Warning Dust. Cutting and grinding stone, concrete and glass throws fine silica dust that causes silicosis, an incurable scarring of the lungs. Always cut wet. Silicon carbide and boron carbide dust are also harmful; crush and grade them wet, and never sweep dry.

Danger Saws and arc furnaces. A large segment saw can snatch work, hands or loose clothing; guard the blade and feed the work on a carriage, not by hand. The carbide arc furnace runs at thousands of amperes, gives off carbon monoxide and blinding light, and sends hot gas jets through the charge: see The Electric Arc Furnace.

  • Pressure in synthetic diamond presses is enormous; a failing anvil explodes like a shell. Such presses need heavy shields.
  • Theft and violence. Diamonds are small and valuable. Recovery of any gem-quality stones needs honest, open record-keeping by several people (Organising a Community).

What this unlocks

Precision Grinding to tenths of a micrometre; fast cutting of building and paving stone (Quarrying and Cutting Stone, Stone Masonry); core drilling for Mining and Tunnelling, Wells and Cisterns and Tunnels and Rock Drilling; fine wire for Copper Wire, lamp filaments and Tungsten and Filament Wire; polishing of Lenses, gems and carbide tools; and, eventually, the high-pressure presses that make diamond grit and cubic boron nitride by the tonne for Machine Tools.

How it was first done

Diamonds were mined from river gravels in India for more than two thousand years, and Indian craftsmen used diamond points to drill hard beads and diamond powder to polish gems. Until the 1720s India was the world's only source; then diamonds were found in the gravels of Minas Gerais, Brazil. In 1866–1871 diamonds were found near Kimberley in South Africa, the first time they had been traced to their source rock, which was named kimberlite. Greased tables to catch the stones came into use there in the 1890s.

In the 1860s the Swiss engineer Rodolphe Leschot set black diamonds in a steel crown to drill rock, the start of diamond core drilling. Diamond wire-drawing dies came into use during the 1800s and became essential for drawing tungsten wire after 1910.

Edward Acheson in Pennsylvania made silicon carbide in 1891 while trying to make diamond, and named it carborundum. Boron carbide was made by Henri Moissan in the 1890s and in industry from the 1930s. In Stockholm, a team at the ASEA company made diamond in a press in February 1953 but did not announce it; on 16 December 1954 Tracy Hall at General Electric made diamond in his "belt" press and his company announced it in 1955. Robert Wentorf at the same laboratory made cubic boron nitride in 1957.