Sodium and potassium are soft, silvery metals so eager to react that they burn in water and must be kept under oil. They are freed by passing a heavy direct current through molten caustic soda in a Castner cell. Sodium lights streets with its yellow lamps, reduces titanium and other stubborn metals, dries solvents, and cools engine valves and reactors. This chapter builds and runs a small Castner cell and gives the strict rules for storing and handling the metal.

Difficulty
●●●●●
Time
A week to dry caustic and build the cell; then about a day of running for each kilogram of sodium at 100 amperes
Steps from zero
17 prerequisites →

You need first

ElectrolysisLye and Potash

This unlocks

—

Objects made here

castner cell
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Salt
  12. Fermentation
  13. Lye and Potash
  14. Bellows
  15. Copper Smelting
  16. The Battery
  17. Electrolysis
  18. Sodium and Potassium Metal

Do them roughly in this order. See it on the tech tree →

Why it matters

Sodium is in every grain of Salt and potassium in every handful of wood-ash Lye and Potash, yet as metals neither exists anywhere in nature. They react with water, with air, with almost everything. That same eagerness is what makes them useful: they pull oxygen and chlorine away from other metals that no fire and no charcoal can free.

This is advanced, dangerous work. Read the whole chapter, especially the dangers, before you begin, and do not attempt it without a steady supply of several hundred watts of direct current and a dry, well-ventilated shed.

How it works

You cannot make sodium with heat and carbon in a simple furnace the way you make iron: at the temperatures a kiln reaches, sodium holds its oxygen too tightly. Electricity forces it (Electrolysis).

Why melt the caustic? In water, the current would make hydrogen instead of sodium, because any sodium formed would react with the water at once. So you melt dry caustic soda (sodium hydroxide), which becomes a clear, oily, conducting liquid at 318 °C. Pass a heavy direct current through it:

  • At the negative electrode (the cathode), sodium ions take electrons and become sodium metal. Sodium melts at 98 °C, so at the bath temperature it is a liquid, and it is lighter than the caustic (about half as dense), so it rises in shining globules and floats.
  • At the positive electrode (the anode), the hydroxide gives up electrons and becomes oxygen and water.

The 50% problem. The water made at the anode drifts into the bath and reacts with some of the sodium, making caustic and hydrogen again. Because of this, a Castner cell can never turn more than half its current into sodium, and real cells give 40–45%. Every 100 ampere-hours therefore gives about 35–40 g of sodium.

Temperature is everything. Run the bath only a few degrees above its melting point, about 320–330 °C. A few tens of degrees hotter and sodium dissolves into the melt, wanders to the anode and burns there; yield falls to almost nothing.

Potassium is made the same way from molten caustic potash, but much less well: potassium dissolves more easily in its melt and is more dangerous to collect. See below.

What you need

Item Size or amount Notes
Iron pot 15–20 cm across, 25–30 cm deep, walls 6 mm or more Cast or heavy welded iron (Metal Casting, Sheet Metal and Rolling). It holds 5–10 kg of caustic
Cathode Iron rod, 3 cm thick Enters through a neck in the pot bottom
Anode Nickel sheet, or iron sheet 3 mm thick, rolled into a cylinder Nickel lasts far longer (Nickel and Cobalt); iron is eaten slowly
Gauze Iron wire gauze, about 1 mm mesh Rolled into a cylinder between the electrodes
Collector Iron tube the size of the gauze cylinder, with a lid and a 5 mm vent Sodium floats up into it
Caustic soda 6–10 kg dry, plus about 2 kg for each kg of sodium From Lye and Potash or Electrolysis, dried as below
DC supply 5–6 V at 50–150 A A low-voltage dynamo (The Generator, Power Supplies and Regulators). Not batteries: you need hundreds of ampere-hours
Heat Charcoal, gas or oil burner under the pot To melt the caustic and hold it at temperature
Perforated iron ladle Bowl 6 cm across, holes 2–3 mm Long handle, 60 cm
Storage oil Dry kerosene or light mineral oil From Petroleum and Refining; never vegetable oil
Safety gear Full face shield, leather gloves and apron, wool clothes, boots Plus a bucket of dry salt or soda ash beside the cell
Lead and zinc scraps A few strips Temperature tests

Dry caustic. Caustic soda made by boiling soda with lime (Lye and Potash) or drawn from a diaphragm cell (Electrolysis) still holds water. Boil the strong solution down in an iron pot outdoors, then keep heating the solid. It melts and bubbles as the last water leaves. When it lies as a quiet, clear oil with no more bubbles, at a heat just short of a dull red glow in the dark, it is dry. Pour it into iron trays to set and break it up into lumps, and store them in sealed iron cans: dry caustic soaks up water and carbon dioxide from the air within hours. Caustic soda made from potash ash contains potassium; sodium for this chapter must come from soda (Soda Ash and Baking Soda).

The Castner cell

Brick firebox Fire in side flues Molten caustic soda 320–330 °C Cathode − iron rod, 3 cm Frozen caustic plug seals the neck Hydrogen vent Collector and lid lift lid, ladle out sodium Molten sodium floats on the caustic Oxygen bubbles rise outside the gauze Iron gauze keeps sodium from the anode Nickel anode + cylinder 2–3 cm from cathode Neck outside the fire, kept cool + −
Fig. 1 The Castner cell in cross-section. Molten caustic soda fills an iron pot. The cathode rises through a neck in the bottom, sealed by a plug of frozen caustic. Sodium forms on the cathode, floats up inside the gauze cylinder and collects in the closed collector, from which it is ladled out. Oxygen rises outside the gauze from the surrounding nickel anode.

The cell is laid out so that the sodium, rising from the cathode, can only go up into the collector, and the oxygen, rising from the anode, can only go up outside it.

Building it

  1. The pot. Cast or weld an iron pot 15–20 cm inside diameter and 25–30 cm deep. In the centre of the bottom, fit a neck: an iron pipe 5–6 cm inside diameter and 12–15 cm long, pointing down.
  2. The cathode. Pass a 3 cm iron rod up through the neck so that its top stands about 10 cm above the pot bottom. Hold it centred with a clamp below the neck, insulated from the pot by a ring of fired clay. Below the neck, bolt a heavy copper strap to it for the negative lead.
  3. The anode. Roll nickel or iron sheet into a cylinder 4–5 cm larger in diameter than the cathode top, so the gap is 2–3 cm, and about as tall as the cathode's exposed part. Hang it from an iron bar across the pot rim, insulated from the pot by clay blocks, so that it surrounds the cathode tip. Its lead is the positive.
  4. The gauze and collector. Roll iron gauze into a cylinder that fits halfway between cathode and anode. Rivet its top to the collector, an iron tube of the same diameter, about 12 cm tall, with a loose lid that has a small vent hole. Hang the collector from the rim so the gauze reaches down to the level of the cathode's base and the collector's mouth sits in the melt. The gauze must not touch either electrode.
  5. The firebox. Build the pot into a brick firebox (Bricks) with a fire space beneath, but leave the neck exposed to the air below. The neck must stay cool enough for caustic to freeze in it.

Starting up

  1. Charge and melt. Fill the pot two-thirds with dry caustic lumps and light the fire. As the caustic melts, some runs down into the neck, meets the cooler pipe and freezes into a solid plug round the cathode. This plug both seals the bottom and insulates the cathode from the pot. Add caustic until the melt stands 3–5 cm above the collector's mouth.
  2. Find the temperature. Dip a strip of lead into the melt on a wire. Lead melts at 327 °C. At the right heat the strip slowly softens and drips; if it melts away at once the bath is too hot. A strip of zinc (melts at 420 °C) must stay quite solid; if it melts, the bath is far too hot. Too cold, and a crust forms on the surface and the edges set.
  3. Switch on the current, starting low, about 20–30 amperes, and building up over half an hour to the working current of 50–150 A for a cell this size. Find your cell's best current by trial: weigh the sodium against the ampere-hours (below) and settle where the yield is highest. Expect 4.5–5 V across the cell. Bubbles of oxygen rise round the anode; hydrogen and a few flashes come from the collector vent. Once running, the current itself makes much of the heat: ease the fire as needed to stay in the lead-test range.

Running and collecting

  1. Every one to two hours, wearing the face shield, lift the collector lid. A layer of molten, mirror-bright sodium floats on the caustic inside.
  2. Ladle it out with the perforated ladle. Molten caustic drains through the holes; the sodium, held together by its surface, stays in the bowl.
  3. Pour it at once into a dry iron mould, such as a shallow trough or a row of tubes 2–3 cm across, and close the lid. Bone-dry is essential: a drop of water in the mould makes it spit and flare.
  4. When the bars are only warm (below about 60 °C), knock them out and drop them straight into a can of dry kerosene or mineral oil.
  5. Top up the cell with dry caustic every few hours: it uses about 1.75 kg of caustic per kilogram of sodium.
  6. Shut down by switching off and letting the cell cool with the lid on; the whole mass sets. To restart, melt it again from the top down.

What to expect: at 100 A, about 35–40 g of sodium an hour, or a kilogram in a little over a day, using about 13 kWh of electricity plus the fuel to keep the bath hot.

Potassium, in outline

Potassium can be made by Davy's original route, electrolysing molten caustic potash (it melts at about 400 °C), and Castner-type cells were tried with it. Yields are poor, because potassium dissolves readily in its own melt and boils away at a lower temperature. Today it is made by passing molten sodium through molten potassium chloride at about 850 °C in a closed steel column; potassium, more volatile, boils off and is condensed. Both routes are for an established works. Potassium is far more dangerous than sodium, and for almost every use sodium does the same job. Make potassium only when you truly need it.

NaK, an alloy of about one part sodium to three of potassium, is liquid at room temperature. It was the first coolant of fast reactors. It is spectacularly reactive and should be made only by people who know exactly why they need it.

The Downs cell, in outline

Big plants since 1924 electrolyse molten salt instead of caustic, with calcium chloride added to lower its melting point to about 600 °C. A graphite anode (Lampblack and Carbon Black) gives off chlorine, sold as a by-product (Chlorine and Bleach); the sodium rises round a ring-shaped iron cathode into a collecting pipe. Current efficiency reaches about 85%, the cell runs for years, and the raw material is cheap salt. It needs good refractories, ruthless exclusion of moisture and a way to use or neutralise a great deal of chlorine. Build it only after the Castner cell works.

Storing and handling

1 Store 2 Cut 3 Fire 4 Destroy scraps tight lid dry oil covers all bright cut face never water dry salt outdoors kerosene or mineral oil, never vegetable oil dry tile, dry knife, tongs not fingers bury it under dry salt, soda ash or sand a few grams at a time in a big bowl of spirit Keep a bucket of dry salt or soda ash beside the cell, the store and the bench at all times.
Fig. 2 Rules for living with sodium. Store it fully under dry oil in a closed can. Cut it on a dry tile with a dry knife, taking only what you need. Smother a fire with dry salt or soda ash, never water. Destroy scraps a little at a time in a large bowl of alcohol, outdoors.
  • Store sodium in a tightly closed glass jar or iron can, completely covered by dry kerosene or light mineral oil, labelled, on a low shelf, far from water, sinks and acids. Not vegetable oil: sodium slowly turns it to soap.
  • Cut it on a dry glazed tile with a dry knife. Fresh-cut sodium is silver and as soft as cold butter; the surface goes dull grey within a minute. Take only what you need and put the rest back under oil at once.
  • Pick it up with dry tongs or forceps, never fingers. Sweat on skin is enough to start a reaction and a deep caustic burn.
  • Scraps and residues: destroy them a few grams at a time by dropping them into a large bowl of ethanol or other spirit (Distillation) outdoors, away from flames. They fizz quietly as they dissolve. When nothing is left, dilute with plenty of water and pour it away.
  • Potassium in storage grows a yellow-orange crust of a compound that can explode when cut or pressed against the metal. Store it under dry oil in small pieces, use it within months, and never cut a piece that has a yellow crust: have it destroyed by someone experienced.

Using sodium

The water demonstration. Drop a piece no bigger than a grain of rice into a wide basin of water outdoors, and stand back behind a sheet of glass. It melts into a silver ball that whizzes over the surface, hissing, sometimes bursting into yellow flame. The water afterwards is weak lye. This one demonstration teaches more respect than any warning.

Sodium lamps. A few grams of sodium sealed into a borate-glass discharge tube gives the yellow street lamp (Arc Lamps, Neon and Fluorescent Lights).

Reducing metals. Titanium tetrachloride dripped onto molten sodium in a sealed steel pot full of argon gives titanium (the Hunter process — compare the magnesium-based Kroll process in Titanium). Henri Sainte-Claire Deville used sodium to make the first cheap aluminium in the 1850s (Aluminium).

Sodium-cooled valves. The exhaust valves of high-powered engines run red-hot. Make the valve stem hollow and fill it about half full of sodium, then weld it shut. In the running engine the sodium melts and sloshes up and down, carrying heat from the head to the stem and into the cooled valve guide. Aircraft engines from the 1930s onward used them (The Internal Combustion Engine, Gliders and Aeroplanes).

Reactor coolant. Liquid sodium carries heat away from a reactor core at ordinary pressure without boiling, up to almost 900 °C. Fast breeder reactors use it (Nuclear Energy (Overview)).

Drying solvents. Thin wire or shavings of sodium in a bottle of ether or benzene take out the last traces of water, needed for anaesthetic ether and for some chemical reactions (Ether, Acetone and Solvents, Anaesthesia).

How to tell it worked

  • Fresh cut: silvery and bright as polished silver, tarnishing to grey within a minute in air. Soft enough to cut with a table knife; squeezes like cold butter.
  • Density: it sinks in kerosene, which is why storage under oil works, but floats on water, fizzing.
  • Flame test: a speck burnt on a wire gives an intense yellow flame (sodium) or a lilac one (potassium; see it through blue glass to hide any yellow).
  • Yield check: weigh a day's sodium against the ampere-hours. Less than 25 g per 100 Ah means the bath is too hot, too wet or the gauze is broken.

Note Troubleshooting. Little or no sodium, the melt foams and flashes → bath too hot. Cut back the fire and current until the lead test is right. Sodium appears, then vanishes → wet caustic. Dry it longer, keep the lids on, and store caustic sealed. Current falls, the cell goes thick → bath too cold, or carbonate building up from carbon dioxide in the air. Raise the heat; replace part of the charge with fresh dry caustic. Caustic leaking from the neck → the neck is too hot. Shield it from the fire, or blow air on it, until the plug sets. Collector fills with grey sludge → oxide and carbonate. Skim it, and keep air out with the lid. Anode thin and holed → iron anodes are eaten; change to nickel.

Dangers

Danger Sodium and potassium burn and explode on contact with water. The reaction makes hydrogen and heat enough to ignite it; a lump the size of a walnut dropped in a sink can burst violently, spraying burning metal and boiling lye. Keep every drop of water away from the cell, the moulds, the storage cans and your hands. Never work in the rain or on a damp floor.

Danger Molten caustic soda at 330 °C blinds and burns to the bone (Lye and Potash). It spits violently if water or wet metal touches it. Full face shield, leather gloves and apron, wool or leather clothing (synthetic fabric melts), boots. Keep a barrel of clean water for rinsing skin, well away from the cell.

Danger Metal fires. Burning sodium cannot be put out with water, foam or carbon dioxide; all make it worse. Smother it under dry salt, dry soda ash or dry sand, poured gently in a thick layer, and leave it buried until cold. Keep a full bucket of one of these beside the cell, the store and the bench at all times.

  • Hydrogen comes from the collector. Vent it upward into open air, and keep sparks and flames away from the vent, or it will pop and flash.
  • Sodium on skin: brush the metal off with something dry, then flood the place with lots of water for 15 minutes and treat as a caustic burn (The First Aid Kit).
  • Potassium's crust can explode. Destroy old potassium rather than cutting it.
  • Heavy current: 100 A at 5 V will not shock you, but a ring or watch strap across the bus bars glows red in seconds. Remove all metal from hands and wrists (Wiring and Electrical Safety).

What this unlocks

How it was first done

On 6 October 1807, at the Royal Institution in London, Humphry Davy passed the current of a large voltaic pile (The Battery) through a lump of slightly damp caustic potash. Small globules of a bright metal appeared at the negative wire; some burst into flame. His cousin wrote that Davy danced about the room in delight. A few days later he made sodium the same way from caustic soda. In 1808 Gay-Lussac and Thénard in Paris made both metals in larger amounts by reacting caustic with red-hot iron.

In the 1850s Henri Sainte-Claire Deville made sodium by heating soda with charcoal and chalk in iron retorts, so that aluminium could be made with it; the price of aluminium fell more than tenfold. The American Hamilton Castner improved this chemical route in 1886, just as the Hall–Héroult process made sodium-reduced aluminium unnecessary. He turned to electricity and patented his molten-caustic cell in 1890; it ran at Oldbury in England and Niagara Falls for decades. The Downs cell, using molten salt, was patented by J. C. Downs in 1924 and replaced it.

Source: content/entries/chemistry/sodium-and-potassium.md