◆ Rebuild

Part 10 · Machines

Packing, Gaskets and Seals

Every machine that holds steam, water, air or oil leaks somewhere. How to stop it — with greased hemp in a stuffing box, gaskets of paper, cork, rubber, lead and copper, springy piston rings, cup leathers, and surfaces lapped so true that they seal by themselves.

Difficulty
●●●●●
Time
An hour to cut a paper gasket or repack a gland; a day to make and fit a set of piston rings; an afternoon to lap a valve
Steps from zero
17 prerequisites →

You need first

The Steam EngineHides and Leather

This unlocks

—
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. The Wheel and Axle
  12. Bellows
  13. The Lathe
  14. Iron (the Bloomery)
  15. Copper Smelting
  16. Blacksmithing
  17. The Steam Engine
  18. Packing, Gaskets and Seals

Do them roughly in this order. See it on the tech tree →

Why it matters

A The Steam Engine whose piston leaks wastes half its steam; a Pumps whose rod leaks sucks air and loses its prime; a hydraulic press that weeps never reaches its pressure; a The Vacuum Pump with a pinhole leak will never make a The Light Bulb. Most early machines that "would not work" were simply leaking.

Some gaps never move — a cover bolted to a cylinder, two pipes joined end to end. These static joints are sealed with a gasket or a paste. Others slide or turn — a piston in its bore, a rod leaving a cylinder, a valve on its seat. These need dynamic seals: packing, piston rings, cup leathers and lapped faces. This chapter covers both, with things you can make: hemp, leather, tallow, paper, cork, rubber, soft metals and grit.

Good seals unlock higher pressures and therefore smaller, stronger engines: the high-pressure The Steam Engine, Boilers and Pressure Vessels, The Internal Combustion Engine engines, Hydraulic Presses and Rams, Ice and Refrigeration and the The Motor Vehicle.

How it works

Why things leak

A fluid leaks wherever there is a path from high pressure to low. Even surfaces that look smooth are, at a tiny scale, hills and valleys; two filed iron faces pressed together touch at only a few high points, and steam slips through the valleys between them.

The key fact: the leak through a thin gap grows with the cube of the gap. Halve the gap and the leak falls to one eighth; make it ten times smaller and the leak falls a thousand times. This is why accuracy matters so much — and why a soft material that fills the gaps works so well. There are only three ways to stop a leak:

  1. Make the gap so small it hardly matters — lapped valve faces, a ground glass stopper, a closely fitted piston.
  2. Fill the gap with something soft that flows into the roughness and is squeezed hard enough to stay there — a gasket, packing, a paste.
  3. Use the pressure itself to close the gap — a cup leather, a piston ring or an O-ring is shaped so that the fluid pushes it harder against the wall. The higher the pressure, the tighter it seals. These are called self-energising seals and they are the cleverest of all.

Squeeze, but not too much

A gasket or packing seals only while it is squeezed harder than the fluid pushes on it. Too little squeeze and it leaks; too much and it is crushed out of the joint, cut through, or — in a moving seal — grips the rod so hard that it burns, scores the rod and wastes power. Most sealing skill is judging this squeeze.

Heat and chemistry

Each sealing material has its limits:

Material Safe up to about Good for Avoid
Vegetable-tanned leather, greased 60–70 °C Cold water, oil, air, hydraulic presses Steam and hot water — it shrinks hard and cracks
Cork 80–100 °C Oil covers, low pressure Steam, high pressure
Paper, oiled or shellacked 100–120 °C Water, oil, low-pressure joints Steam above a few bar
Vulcanised rubber (Rubber) 80–120 °C Water, air, low-pressure steam Oil and petrol swell and rot it
Hemp or flax with tallow and graphite 150–180 °C Steam glands up to about 8–10 bar, pumps Dry running; superheated steam
Lead 250 °C Acids, water, steam flanges in a groove Vibration (it creeps)
Annealed copper 400 °C and more Steam, exhaust, high pressure Joints that must be broken often

What you need

Item Use Source
Hemp or flax yarn Braided packing Flax, Hemp and Linen, Cordage and Rope
Tallow, beeswax Lubricating and filling packing and leathers Rendered animal fat; Beekeeping
Graphite powder Mixed into packing and jointing paste Pencils and Chalk
Strong paper or card Gaskets for water and oil Paper
Cork sheet Oil-tight covers Bark of the cork oak
Vulcanised rubber sheet and cord Gaskets, O-rings Rubber
Sheet lead and copper, 0.5–2 mm Metal gaskets Lead, Copper Smelting
Thick vegetable-tanned leather Cup leathers, flap valves Hides and Leather
Linseed oil, chalk Jointing paste Oils and Pressing, Lime
Emery and tripoli, graded Lapping Abrasives and Grinding Stones
Cast-iron piston-ring blanks Piston rings The Blast Furnace and Cast Iron, The Lathe
Tools Sharp knife, hollow punches, ball-faced hammer, wooden tamping sticks, packing hook (a bent wire with a sharp corkscrew tip), lathe Machine Tools

Where to find it

  • Hemp and flax fibre come from retted stalks (Flax, Hemp and Linen). Long, strong line fibre makes the best packing; short tow will do if it is twisted firmly.
  • Cork is the thick, spongy outer bark of the cork oak, an evergreen oak of the western Mediterranean (Portugal, Spain, North Africa). Bark is stripped from living trees every nine or ten years without killing them. Elsewhere, use leather, paper or rubber instead.
  • Graphite is a soft, black, greasy mineral that leaves a grey mark on paper and feels slippery between the fingers; it occurs in veins and flakes in old metamorphic rocks such as schist and marble.
  • Lead is smelted from galena — heavy, bright grey cubes that split into smaller cubes (Lead). Copper comes from native copper or its ores (Copper Smelting).
  • Linseed oil is pressed from flax seed (Oils and Pressing). It is a drying oil: it slowly hardens in air, which is exactly what you want in a jointing paste and exactly what you do not want in a bearing (Bearings and Lubrication).

Method 1: Packing a stuffing box

Wherever a rod slides or a shaft turns through the wall of a cylinder or pump, it passes through a stuffing box: a deep, wide cup round the rod, filled with rings of soft packing, and squeezed by a sleeve called the gland (or follower) pulled in by two or three studs and nuts.

Cylinder end steam or waterunder pressure Packing ringsbraided hemp, tallow and graphite Glandbronze sleeve that squeezes the packing Studs and nutstighten evenly, one flat at a time Rodstraight, round and polished;slides or turns through the box Stuffing boxbore = rod + 2 × packing size Joints staggeredeach ring's 45° cut turned round from the last close-fitting throat bush squeeze
Fig. 1 A stuffing box in section. Rings of braided packing fill the space round the rod; the gland, pulled in by its studs, squeezes them so they press against the rod and the box wall. The joints of the rings are staggered so there is no straight path for a leak.

Make the box the right size

Rod diameter Packing size (square) Number of rings
10–18 mm 5–6 mm 4–5
18–25 mm 6–8 mm 5
25–50 mm 8–10 mm 5–6
50–75 mm 10–12 mm 6
75–100 mm 12–16 mm 6–8

The box bore is the rod diameter plus twice the packing size. Its depth holds the rings plus room for the gland to enter 1–2 cm. The bottom of the box and the gland's inner end should fit the rod closely (0.2–0.5 mm clearance) so that the packing is not squeezed out through the gap. Bronze at the bottom of the box and in the gland is best; it will not score a steel rod if they touch.

Make the packing

  1. Braid it. Take 4 or 8 strands of hemp or flax yarn and plait them into a square braid of the size you need (a four-strand round plait pressed square between two boards also works). Braid firmly: loose packing compacts and needs constant tightening.
  2. Soak it. Melt 4 parts tallow with 1 part beeswax and stir in 1 part fine graphite. Draw the braid slowly through the hot mixture, let it soak a minute, then pull it through a hole in a board to strip the excess. Let it cool. For cold-water pumps, tallow alone is fine.
  3. For hot steam rods, use more graphite and less fat. Tallow breaks down in steam into fatty acids that slowly eat iron, so wipe and repack regularly. Once you have mineral oil (Petroleum and Refining), use it with graphite instead of tallow.

Fit it

  1. Remove all old packing with the packing hook. Clean the box and check the rod: it must be straight, round and polished. A scored rod chews through any packing; polish it with fine emery and oil, then tripoli.
  2. Cut rings, don't wind a spiral. Wrap the packing round a spare bar of the same diameter as the rod and cut straight across all the turns at a 45° slant with a sharp knife. Each ring then has a long sloping joint that closes neatly.
  3. Fit one ring at a time. Open it sideways (twist, don't pull it straight), slip it round the rod, and push it to the bottom of the box with a split wooden bush or a flat stick. Tamp it firmly.
  4. Stagger the joints: turn each ring so its joint is a quarter-turn (with 4 rings) or a third of a turn (with 3 or 6) from the one before. Joints in a line make a leak path.
  5. Fit the gland and pull it in evenly, a half-turn on each nut in turn, until it just touches the packing. Then tighten each nut only one flat of the nut (a sixth of a turn) more.
  6. Run it in. Start the machine. A new gland should leak a little at first. Tighten one flat at a time, a few minutes apart, as it warms and beds in.

How tight? A water-pump gland should drip slowly — about one drop every second or two. That water cools and lubricates the packing; a bone-dry pump gland is too tight and will soon burn. A steam gland, once hot, should show at most a faint damp film on the rod and no wisps of steam. If you can no longer turn a pump shaft by hand, or the gland gets too hot to touch, slacken it.

Method 2: Gaskets for bolted joints

A gasket is a thin sheet of soft material clamped between two faces. It fills their roughness and small errors of flatness.

  1. Make the faces as flat as you can. File or scrape them on the surface plate (Machine Tools). A gasket fills roughness, not big errors: the flatter the faces, the thinner the gasket and the better it holds.
  2. Choose the thinnest gasket that will fill the faces: paper 0.3–0.8 mm, cork or rubber 1.5–3 mm. Thick gaskets creep under the bolts, loosen and blow out.
  3. Cut it. Lay the paper over the face and tap lightly round the edge with the round face of a hammer: the sharp edge of the metal cuts the paper cleanly. Tap the bolt holes the same way, or cut them with a hollow punch (a short piece of sharpened tube). Make the bore of the gasket a little bigger than the bore of the pipe or cylinder so no edge sticks into the flow.
  4. Dress it. For water joints, smear paper with tallow or soak it in thin shellac (Glues and Adhesives) and let it get tacky. For oil joints, use paper or cork dry or with a smear of shellac. Rubber goes in clean and dry.
  5. Tighten in a star pattern — opposite bolts in turn, a little at a time, three or four rounds — so the faces come together evenly. Bolts on a pressure joint should be no more than about 4–6 bolt diameters apart; farther apart, the flange bends between them and leaks.
  6. Re-tighten after the first heating. Paper and fibre settle.

Metal gaskets take heat and pressure that soft ones cannot.

  • Copper rings for steam pipes, plugs and engine heads. Copper hardens as you squeeze it; soften it first by heating to a dull red and dropping it in water (copper, unlike steel, is softened by quenching). A used copper washer can be softened again the same way and reused.
  • Lead suits acid lines (Sulfuric Acid) and cold-water mains. Lay a ring of lead wire in a shallow groove turned in one flange; the groove stops it creeping out.

Jointing pastes seal screwed pipe threads and rough cast-iron joints.

  • Linseed oil and chalk, worked to a stiff putty, with a little graphite; wind a few strands of hemp round the thread in the direction it screws in, smear with paste and screw up. It hardens in days but can still be unscrewed.
  • The rust joint — the old engineer's permanent seal for cast-iron joints that never need opening. Mix about 100 parts clean iron filings or borings with 1 part sal ammoniac and half a part of powdered sulfur (by weight), and wet it with water just before use. Caulk it hard into the joint with a blunt chisel. It rusts into solid iron oxide over a few days and holds steam and water for decades. It will also crack a thin casting if packed too hard; caulk in layers.

Warning Old pipe-fitters used red lead (lead oxide) in linseed oil on hemp. It seals beautifully and it is a poison that builds up in the body. Use chalk and graphite instead. If you must use red lead, never let it touch food, wear gloves, and wash before eating (Lead).

Method 3: Piston rings

A piston packed with hemp works, but the packing wears, dries and must be renewed. The lasting answer is the piston ring: a thin, springy ring of cast iron set in a groove round the piston. It is made a little too big for the bore, then cut through once, so when it is squeezed into the cylinder it presses outward all round. The fluid gets behind it in the groove and presses it harder still against the wall and the side of the groove — a self-energising seal. Two or three rings in a row stop nearly all leakage.

1. Turn it 3% largedashed line = the bore 2. Cut out a pieceabout π × the oversize 3. Clamp closed, turnso it is round when closed 4. Spring it in the boreend gap 0.3–0.4% of bore lathe tool:light cut clamp gap Pressure Ring in its groove gas gets behind it and pressesit out against the wall anddown against the groove side side clearance 0.03–0.05 mm Cylinder wall bored and lapped Piston
Fig. 2 Making a piston ring. A ring is turned 3% larger than the bore, a piece is cut out of it, and it is clamped closed and turned again so that it is truly round when squeezed into the cylinder. In the piston it sits in a groove with a tiny side clearance and a small gap at the ends.
  1. Cast a sleeve of fine-grained grey cast iron, a little bigger than the bore and long enough for several rings (The Blast Furnace and Cast Iron, Metal Casting). Grey iron is springy enough when thin and wears beautifully against a cast-iron cylinder.
  2. Bore and turn it on the The Lathe: inside to the bore minus twice the ring's radial thickness; outside to about 3% more than the cylinder bore (a 100 mm bore wants rings turned to about 103 mm). Radial thickness: about one twenty-fifth of the bore (4 mm for a 100 mm bore). Part off rings 3–6 mm wide.
  3. Cut the gap. Saw out a slanting piece so that when the ring is squeezed to the bore its ends almost meet. The piece to remove is about π times the oversize: 3 mm × 3.14 ≈ 9.4 mm, minus the end gap.
  4. Turn it round again. Clamp the ring closed to bore size between two plates (or in a split sleeve) and take a light finishing cut on the outside. Now, when it is in the cylinder, it touches all round instead of only at the ends.
  5. Check the end gap with the ring pushed squarely into the cylinder: about 0.3–0.4% of the bore (0.3–0.4 mm on 100 mm). Too small and it closes up and jams when hot; too big and it leaks.
  6. Groove the piston: a groove the ring width plus 0.03–0.05 mm (side clearance), and a little deeper than the ring's radial thickness so the ring never bottoms. Stagger the gaps of the rings round the piston.
  7. Fit carefully. Spread a cast-iron ring only just enough to slip over the piston — slide three thin strips of tin under it as ramps. Overspread it and it snaps.

Method 4: Cup leathers and O-rings

For cold water, oil and air at high pressure, the cup leather (U-leather) is hard to beat: a ring of thick leather moulded to a U section, set with its open side facing the pressure, so the liquid pushes its lips harder against the wall. How to mould it is in Hydraulic Presses and Rams; pump buckets are in Pumps. Keep leathers supple with tallow and beeswax, and never let them run in hot water.

Once you have vulcanised rubber, the O-ring is the simplest seal of all: a ring of round rubber cord sitting in a square-cut groove. Make the groove depth about 80% of the cord thickness, so the ring is squeezed by a fifth, and the groove width about 1.4 times the cord thickness, so pressure can push the ring to one side and wedge it into the corner. Mould rings by vulcanising rubber in a two-part ring mould, or join a length of cord with rubber cement and cure the joint (Rubber). O-rings seal water, air and (with the right rubber — oil-resistant nitrile, Synthetic Rubber Works (Overview)) oil, both standing still and on slow-moving rods.

Gasket joint Gasketpaper, cork, rubber, lead or copper bolts 4–6 diameters apart, tightened in a star pattern O-ring pressure groove 80% of cord depth, 1.4 × wide; pressure wedges the ring into the far corner groove rubber ring Cup leather Leatheropen sideto pressure piston Lapping a valve twist back and forth,lift, move round, repeat Valve Seat45°, 1–3 mm wide;fine emery in oil
Fig. 3 Four seals. A paper gasket between bolted flanges; an O-ring squeezed in its groove, pushed into the corner by pressure; a cup leather whose lips are pressed outward by the liquid; and a valve being lapped into its conical seat with fine grit and oil.

Method 5: Lapping surfaces to seal by themselves

When two hard surfaces are made true enough, no gasket is needed: the gap is too small to leak. Lapping is how you get there — rubbing the two parts against each other, or against a true plate, with fine grit in oil, so the high spots wear away until they fit.

A conical valve in its seat (safety valves, check valves, pump and engine valves):

  1. Make the seat a narrow cone at 45° (or 30°), only 1–3 mm wide. A narrow seat presses harder per square centimetre and seals better than a wide one.
  2. Smear a little fine emery mixed with oil on the valve face. Put the valve in its seat with a light spring or light hand pressure.
  3. Turn it back and forth through a quarter turn ten or twelve times, lift it, turn it to a new position and repeat. Lifting lets grit get back between the faces and stops you grinding rings into them.
  4. After a few minutes, wipe clean and look: a good lap shows an unbroken dull-grey ring all the way round, on both valve and seat. Finish with a finer grade (flour emery or tripoli) for a minute.
  5. Wash out every trace of grit with oil or paraffin. Grit left in a machine goes on lapping everything it touches.

Flat faces (steam-engine port faces, slide valves, pump plates): lap each on a true cast-iron plate (Machine Tools) charged with fine emery and oil, moving in figure-eights and turning the part often, then against each other. This is how the oscillating valve of the small The Steam Engine is made steam-tight. Ground glass joints are made the same way (Laboratory Glassware).

How to tell it worked

  • The pencil test for a valve: draw six soft-pencil or soot lines across the seat, drop the valve in and give it one small twist. Every line should be cut through all the way round.
  • The paraffin test: stand a lapped valve in its seat, fill above it with paraffin or thin oil, and watch underneath. A good valve holds for minutes without a drop.
  • Soapy water brushed on air, gas and vacuum joints shows a leak as a growing bubble.
  • The chalk wash: paint water joints with whitewash (Lime) and let it dry. A weeping joint shows as a dark wet patch long before it drips.
  • Steam: hold a cold, polished steel blade or a mirror near the joint (never your hand). A leak fogs it.
  • Pressure decay: pump up a vessel, close it, and see how far its gauge falls in an hour, before and after your repair.

Note Troubleshooting. Gland leaks however much you tighten it → rod scored, bent or worn oval; packing too small; or old hardened packing left at the bottom. Strip it, check the rod, repack with fresh rings. Gland hot and dry, shaft stiff → too tight; slacken until it drips, then retighten gently once warm. Gasket blows out on one side → bolts too far apart, tightened unevenly, or gasket too thick. Use thinner gasket and tighten in a star pattern. Joint leaks again after heating → gasket settled; re-tighten when cool. Paper over about 120 °C chars — use copper or fibre. Rings stuck in their grooves → carbon and burnt oil; clean the grooves, check side clearance. Valve still weeps after lapping → seat too wide, valve guide worn so it does not land square, or a pit in the face. Narrow the seat, bush the guide, or recut and lap again. Cup leather fails quickly → it ran dry, met hot water, or faced the wrong way. The open side of the U must face the pressure.

Dangers

Danger Never tighten, loosen or repack anything that is under pressure. A stud snapping or a gasket blowing on a live steam joint sprays scalding steam over the face and hands. Shut off, let the pressure fall to zero, and open a drain cock before you touch a gland or flange. Steam from a fine leak is invisible for the first few centimetres and hot enough to cut skin to the bone; feel for it with a stick or a broom straw, never your hand. High-pressure oil or water from a pinhole can pierce the skin and inject itself into the hand — a small-looking wound that can lose the hand (Hydraulic Presses and Rams). Get it seen at once.

Danger Asbestos. Industrial engineers once made packing and gaskets of a white, silky, fibrous mineral called asbestos, because it does not burn. Its dust causes lung scarring and cancers that appear 20–40 years later and kill. Do not use it, and do not grind, saw or brush out old gaskets that might contain it. Use graphite, copper and hemp instead.

  • Lead in gaskets and red lead in paste are poisonous; handle with gloves and wash.
  • Oily packing waste and rags soaked in linseed oil can heat themselves and catch fire. Spread them out or burn them.
  • Lapping grit in the eye scratches it; wear eye protection when lapping fast on a wheel.

Going further

How it was first done

Thomas Newcomen's engine of 1712 sealed its piston with a disc of leather and a layer of water lying on top. When James Watt built a separately condensed engine in the 1760s, steam leaked past every imperfect cylinder until John Wilkinson's boring machine (1774) gave him cylinders round enough to seal with greased hemp packing; Watt wrote that a 50-inch cylinder did not err "the thickness of an old shilling" in any part. Stuffing boxes with hemp packing and glands became standard on engines and pumps through the 1700s.

Joseph Bramah's hydraulic press of 1795 leaked until his foreman Henry Maudslay devised the self-tightening U-shaped leather collar. Vulcanised rubber (Goodyear and Hancock, 1840s) brought rubber gaskets and valves. John Ramsbottom, a locomotive engineer in England, introduced split, springy metal piston rings in the early 1850s; cast-iron rings soon replaced hemp packing on pistons everywhere. In 1899 the Austrian engineer Richard Klinger made compressed asbestos-fibre gasket sheet, used for most of the 20th century until its dangers became clear. The O-ring was patented by Niels Christensen in the United States (filed 1937, granted 1939), and in the Second World War it became the standard seal of aircraft hydraulics.

Source: content/entries/mechanics/packing-and-seals.md