◆ Rebuild

Part 5 · Cloth and Clothing

Cotton

Grow cotton in a warm, frost-free season, pick the fluffy bolls, strip the seeds out with a roller gin, and fluff the fibre with a bow and cards ready to spin. Cotton makes soft, washable, cheap cloth — and the hunger for it drove the first factories.

Difficulty
●●●●●
Time
5–7 months from sowing to the last picking; ginning a kilogram of fibre takes about two days by hand, much less on a roller gin
Steps from zero
2 prerequisites →

You need first

Farming from Seed

This unlocks

Menstrual Pads, Toilet Paper and Continence Care

Raw materials

cottonkapokwood ash
The full path from nothing — 2 steps before this one
  1. Stone Tools
  2. Farming from Seed
  3. Cotton

Do them roughly in this order. See it on the tech tree →

Why it matters

Cotton is the most comfortable everyday cloth there is: soft, absorbent, cool in heat, easy to wash and boil, and cheap once you can grow and process it in bulk. It makes underclothes, shirts, sheets, towels, bandages and dressings (Wound Care and Antiseptics), sanitary pads (Menstrual Pads, Toilet Paper and Continence Care), filter cloths, lamp and candle wicks (Lamps and Candles), and the soft "cotton wool" used to plug sterile flasks (Penicillin). Cotton thread, like silk, was wrapped round early electric wires to insulate them (Copper Wire), and a charred cotton thread made the first long-lasting The Light Bulb filament.

Unlike Flax, Hemp and Linen, cotton needs no retting: the fibre grows as a soft fluff on the seed, ready to use. The only hard part is getting the seeds out — and the machine that solved that problem changed world history.

How it works

Cotton (Gossypium) is a shrub of the mallow family. After each flower fades, its base swells into a green capsule called a boll, about the size of a walnut. Inside, 25–45 seeds sit in three to five compartments (locks). Each seed grows thousands of hairs from its skin. A single hair is one long, hollow cell of almost pure cellulose (the same material as linen and paper).

When the boll ripens, it dries and splits open, and the hairs dry and collapse into flat, twisted ribbons. That natural twist is the secret of cotton: the fibres hook and grip each other when spun, so even though they are short, they make a strong yarn. Fibre length is called staple:

  • Short staple (under 2.5 cm) — coarse, harder to spin.
  • Medium staple (2.5–3 cm) — most upland cotton.
  • Long staple (3–5 cm) — sea-island and Egyptian cotton, the finest and strongest yarn.

Many cottons also have a short fuzz (linters) stuck tightly to the seed under the long fibre. Fuzzy-seeded cotton is much harder to gin than smooth, "black-seed" cotton — which matters when you build the gin.

By weight, a boll of picked seed cotton is about one third fibre (lint) and two thirds seed.

Flowercream, turns pinknext day; 60–70 daysafter sowing Green bollwalnut-sized, insidethree frilled bracts;50–60 days to ripen Open boll3–5 white locks;pick in dry weather,husk stays on plant One seedthousands of hairs,2–5 cm long; about athird of the weight FROM FLOWER TO FIBRE
Fig. 1 The cotton plant. A creamy flower becomes a green boll in about two months; the boll splits and shows four or five white locks, each holding several seeds wrapped in long fibre.

What you need

Item Notes
Cotton seed A double handful sows about 100 m²
Land A warm, sunny plot; 100 m² gives roughly 15–30 kg of seed cotton, or 5–10 kg of fibre in a good year
Picking bags Cloth or basket, carried at the waist
Roller gin Two hardwood rollers 2–3 cm thick in a frame, geared to turn opposite ways — see below
Bow A cotton-beater's bow, about 1–1.5 m long, strung with gut or sinew, and a wooden mallet
Hand cards Like wool cards, but with finer, closer teeth (Wool)

Where to find it

Climate. Cotton needs a long, hot, frost-free growing season — at least 180–200 days without frost, with nights above about 15 °C for most of that time, plenty of sun, and soil warmer than about 16–18 °C at sowing (warm to the bare hand at seed depth early in the morning). That means the tropics, subtropics and warm-temperate lowlands: roughly between latitudes 40° north and 35° south. It needs water while growing (about 500–1,200 mm of rain, or Irrigation) and dry weather when the bolls open, or the fibre rots.

Finding seed. Four cotton species were domesticated separately, in Mexico, South America, India and Africa. Cotton escapes from fields and grows as a perennial shrub or small tree along tropical coasts, roadsides and old farms; in frost-free places, old plantings survive for years. Seed may also be found in old seed stores, bales of raw cotton and mattress stuffing (raw "seed cotton"), or as cottonseed sold for animal feed or oil — though seed for oil is often delinted with acid, and seed that was heated or crushed will not grow. Test a few in damp cloth: good seed sprouts in a week in warmth.

Identifying cotton. A bushy shrub 1–2 m tall (taller as a perennial), with broad leaves lobed like a hand (three to five lobes), and large cup-shaped flowers, cream or pale yellow, often with a purple spot at the base, which turn pink or red the day after opening and drop. Below each flower are three large, frilled, leafy bracts. The boll is pointed, green and leathery until it opens.

Other seed fibres do not spin well but are excellent stuffing:

  • Kapok, the silky floss of the tropical kapok tree, is light, water-repellent and floats for weeks: the traditional filling for life jackets (Life Jackets, Lifebuoys and Lifeboats), pillows and mattresses (Mattresses and Upholstery).
  • Milkweed floss (temperate North America), cattail fluff and cotton grass (bogs of the north) are similar. Mixed with a little wool or cotton they can be spun, but the yarn is weak.

Step by step

1. Grow it

  1. Prepare the ground like any row crop (Farming from Seed): deep, well-drained, fertile soil. Cotton tolerates some salt and some drought once established, but not frost or waterlogging.
  2. Soak the seed overnight in warm water. Fuzzy seeds stick together; rubbing them in a little wet ash or dung separates them.
  3. Sow when the soil is warm, 2–3 cm deep, 3–5 seeds together every 30–45 cm along rows 90–100 cm apart. They sprout in 5–10 days.
  4. Thin to the 1–2 strongest seedlings per spot when they are a hand high.
  5. Weed for the first two months. Hoe soil up round the stems.
  6. Water well while flowering and while the bolls swell, then let the field dry out as the bolls begin to open.
  7. Flowering starts about 60–70 days after sowing and continues for weeks. Each boll takes 50–60 days from flower to opening.

Tip Pinch the tops of the main stems when the plants are about 1–1.2 m tall, near the end of the season. The plant then puts its strength into ripening the bolls it already has instead of making new ones that frost will kill.

2. Pick it

  1. Pick as the bolls open, every week or two, over 6–10 weeks. Do not wait for them all.
  2. Pick in dry weather, after the dew has dried. Grip each lock at its base and pull it out of the dry husk in one piece, leaving the husk on the plant. Leaves, husk fragments and dirt in the cotton are hard to get out later.
  3. Keep grades apart: clean, white, fully open locks are your first grade; stained, rain-damaged or bug-eaten locks are second grade, for stuffing and wicks.
  4. Dry the seed cotton in the sun for a few days, spread thinly, before storing it in a dry, airy place. Damp seed cotton heats, moulds, and yellows. Store it clear of fire.

Keep seed from the best plants — tall, with many large bolls and long, white fibre — for next year (Saving Seed and Breeding Plants).

3. Gin it — separating fibre from seed

By hand. Pull the fibre off each seed with your fingers, or roll the seed under a smooth iron or wooden rod on a flat stone, pushing the fibre away from the seed. It works, but one person cleans only about half a kilo of fibre a day. That is why cotton was a luxury in most places until the gin.

The roller gin (churka). This is the machine to build first.

ROLLER GIN (CHURKA) best for smooth, long-staple seed Seed cottonfed in small tufts Hardwood rollers2–3 cm thick, turningtowards each other Clean lintthrough the gap Seedstoo big for the gap,drop on the feed side crank one roller; wooden screw threadscut on the roller ends turn the other SAW GIN (WHITNEY TYPE) for fuzzy seed and large amounts Grid of barsslots ~3 mm Toothed drumhooks fibre through slots Hopper seedsout Brush drumturns faster,sweeps lint off
Fig. 2 Two ways to gin cotton. In the roller gin, two rollers turning towards each other pull the fibre through the narrow gap and leave the seeds behind. In the saw gin, hooked teeth on a drum pull fibre through slots too narrow for seeds, and a brush sweeps the fibre off.
  1. Make two rollers of straight-grained hardwood (or iron), each about 2–3 cm thick and 25–30 cm long, smooth and perfectly round — a The Lathe helps. Fine grooves along their length help them grip.
  2. Mount them one above the other in an upright wooden frame, the gap between them narrower than a seed (about 1 mm, or just touching). Their ends turn in holes in the frame posts, greased with fat.
  3. Make them turn in opposite directions. The simplest way is to cut matching wooden screw threads (worm gears) on the ends of the two rollers so that turning one turns the other the other way. A crank handle on one roller drives both (see Gears and Cranks, Cams and Linkages). Without threads, fit a crank on each roller and have two people turn them.
  4. Feed small tufts of seed cotton into the gap with one hand while turning with the other. The rollers grab the fibre and pull it through; the seeds cannot fit, and drop on the feeding side. Clean fibre comes out on the far side.

A well-made roller gin cleans several times as much as hand-picking. It works best with smooth-seeded, long-staple cotton. With fuzzy-seeded cotton, the fuzz drags seeds into the gap and the gin jams or crushes them; work more slowly and pick off crushed seeds.

The saw gin (Whitney's cotton gin). For fuzzy-seeded cotton in quantity, build a drum gin:

  1. A wooden drum 20–30 cm across carries rows of hooked iron wire teeth, or circular saw-toothed iron discs spaced about 2 cm apart.
  2. Above it, a hopper of seed cotton sits on a grid of iron or hardwood bars with slots just wide enough for the teeth to pass through but too narrow for seeds (about 3 mm).
  3. As the drum turns, the teeth hook the fibre and drag it down through the slots, tearing it off the seeds. The seeds stay in the hopper and fall out of an opening at the bottom.
  4. A second drum fitted with stiff brushes, turning in the opposite direction and faster (gear it up 3–4 times), sweeps the fibre off the teeth and blows it out.

A hand-cranked saw gin clears tens of kilograms of seed cotton a day; a horse or water-powered one (Draft Animals and Harness, The Waterwheel) far more. It roughens long fibres a little, so the roller gin is still better for fine, long cotton.

4. Clean and fluff the fibre (bowing)

Ginned cotton is still matted and full of leaf bits. The ancient way to open it is the bow:

  1. Make a bow about 1–1.5 m long of springy wood, strung with gut or twisted sinew (Cordage and Rope), and hang it from a cord so it floats just above a pile of cotton on a mat or sheet.
  2. Lower the string into the cotton and strike it near one end with a wooden mallet, or pluck it hard. The string twangs and vibrates through the fibres, flinging them up into the air as a fluffy cloud while heavier dirt and seed fragments drop out.
  3. Move the bow slowly through the pile. A practised bower turns a heap of matted lint into soft, even fluff.

5. Card and roll punis

Card the fibre with fine hand cards, as for wool (Wool), using a light touch: cotton is short, and heavy carding breaks it. Lift off the carded sheet and roll it tightly round a thin smooth stick (a skewer or knitting needle), then slide out the stick. The result is a puni — a firm, finger-thick tube about 20 cm long — the classic form for spinning cotton.

Cotton is spun with much more twist than wool, because its fibres are short. A dropped spindle drags short fibres apart, so cotton is usually spun on a light support spindle whose tip rests in a little bowl, or on a The Spinning Wheel. See Spinning and Weaving Cloth.

How to tell it worked

  • Good lint is white or creamy (some old varieties are naturally brown or green), soft, and free of seed pieces. Pull a tuft gently apart between two hands: fibres at least 2.5 cm long mean a good spinning cotton.
  • A good gin delivers lint with no broken seeds and drops whole seeds, almost bare, on the feeding side.
  • Well-bowed cotton is fluffy and even, without visible clumps or "neps" (tiny white knots).

Note Troubleshooting. Plants grow but few bolls form → too much nitrogen or water (all leaves, no fruit), or nights too cold. Use less manure, and sow earlier on the warmest ground. Bolls rot before opening → rain or humid weather at ripening, or insects. Choose an earlier variety; space plants for air movement. Gin jams → seeds too damp (dry the seed cotton in the sun first), feed too fast, or rollers too far apart. Lint full of crushed seed → rollers too tight or too slow; fuzzy seed in a roller gin. Yarn keeps pulling apart → not enough twist, or the fibre is too short; use a support spindle and more twist.

Dangers

Danger Cotton fibre burns fast. Loose lint, ginning dust and seed cotton catch fire from a spark and burn explosively in a cloud. Damp, packed seed cotton can heat up by itself and smoulder deep inside a heap. Keep fire, lamps and smoking far away from gins and stores, dry cotton fully before storing, and keep water and sand at hand.

  • Cotton dust in the lungs ("brown lung", byssinosis): years of breathing gin and carding dust cause a tight chest and cough, worst at the start of each working week. Gin and bow outdoors or with good airflow, and wear a damp cloth over nose and mouth.
  • Cottonseed is poisonous to eat raw. It contains gossypol, which damages the heart and liver and causes infertility in people, pigs and poultry. Cattle tolerate modest amounts. Do not eat the seed; oil pressed from it must be properly refined before eating (Oils and Pressing).
  • Gin injuries. Saw gins and rollers catch fingers and sleeves. Never reach into a running gin; feed with a stick.
  • Pests. Boll weevils and bollworms can destroy a crop. Burn or plough under old cotton stalks after harvest to break their life cycle (Pests and Plant Diseases).

What this unlocks

Spin it (Spinning and Weaving Cloth, The Spinning Wheel) and weave it (The Loom) into cloth for Making Clothes, bandages for Wound Care and Antiseptics, and wicks for Lamps and Candles. Cotton thread insulates Copper Wire and makes The Light Bulb filaments. Cotton lint and linters are nearly pure cellulose — the raw material of celluloid and rayon (Early Plastics, Rayon and Nylon) and of fine Paper. Above all, cotton's short fibre and huge demand made it the first fibre spun and woven by machine (Textile Machinery).

How it was first done

Cotton was domesticated at least four times independently. The oldest known cotton fibres, preserved by copper salts inside a bead, come from a burial at Mehrgarh in Pakistan, roughly 7,000–8,000 years old; by about 4,500 years ago the cities of the Indus Valley were growing and weaving cotton on a large scale. In the Americas, cotton was grown in coastal Peru and in Mexico more than 5,000 years ago, and some of the oldest cotton cloth anywhere comes from Huaca Prieta in Peru. The Greek historian Herodotus wrote in the 5th century BC of Indian "trees that bear wool finer than sheep's". The roller gin was used in India by the first millennium AD and spread with cotton across the Islamic world and China. In 1793 Eli Whitney built his toothed cotton gin in Georgia, USA, which made fuzzy-seeded upland cotton profitable. It also made slavery on cotton plantations vastly more profitable, and the number of enslaved people in the American South grew several times over in the following decades — a reminder that a machine's effects depend on the society that uses it. The demand for cotton yarn and cloth then drove the invention of the spinning and weaving machines of the Industrial Revolution.

Source: content/entries/textiles/cotton.md