◆ Rebuild

Part 3 · Metals

Bronze

Copper with about one-tenth tin. Bronze melts lower, casts better and hammers far harder than copper — hard enough to replace stone tools for good. This chapter covers finding and smelting tin, alloying, casting in stone, clay and lost-wax moulds, and hardening the edge.

Difficulty
●●●●●
Time
A day to smelt tin; a day to alloy and cast; several days to make and dry lost-wax moulds
Steps from zero
12 prerequisites →

You need first

Copper Smelting

This unlocks

Bearings and Lubrication

Objects made here

cruciblecasting mould
The full path from nothing — 12 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Copper Smelting
  13. Bronze

Do them roughly in this order. See it on the tech tree →

Why it matters

Pure Copper Smelting is soft. A copper axe bends on hardwood knots and a copper knife dulls quickly. Add about one part of tin to nine parts of copper and the result — bronze — is a different material: it melts about 80 °C lower, flows into the finest details of a mould, and after hammering can be roughly as hard as unhardened mild steel. For two thousand years, bronze was the best material people had for axes, chisels, saws, knives, sickles, needles, nails, hinges, pots, mirrors and bells.

For you, bronze is the bridge between your first copper and Iron (the Bloomery). Iron ore is common and iron is cheaper in the end, but iron must be smelted in a much hotter furnace and forged rather than cast (see Blacksmithing). Bronze can be cast into almost any shape with skills you already have: gear wheels, bearings, valves, pump bodies and pipe fittings — machine parts that resist corrosion and wear. Bronze remains a metal of choice for bells, ship propellers and fittings, and bearings even today.

How it works

An alloy is a mixture of metals melted together. When tin atoms sit among copper atoms, they are a slightly different size and jam the layers of copper atoms so they cannot slide past each other as easily. That is what makes bronze harder and stronger.

Tin also lowers the melting point. Copper melts at 1,085 °C; a bronze with 10% tin is fully liquid at about 1,000 °C. Tin melts at only 232 °C — on a cooking fire.

How much tin you add changes everything:

sheet, wire TOOLSaxes, knives, gears castings, bearings bells mirrors 0%5%10%15%20%25%30% more tin: harder, paler, more brittle Melting point copper 1,085 °C · 10% bronze about 1,000 °C · tin alone 232 °C tin in the alloy, by weight
Fig. 1 How the amount of tin changes bronze. About 10% is the all-round tool metal.
Tin (by weight) Properties Uses
0% (pure copper) Soft, very ductile, conducts electricity best Wire, sheet, pots
2–5% A little harder, still easy to hammer cold Sheet, wire, rivets, pins
8–12% Casts well, hammers hard, tough Axes, chisels, knives, saws, sickles, gears
13–16% Harder, but cracks if hammered much cold Cast parts, bearings
20–25% Very hard and brittle; rings beautifully Bells, cymbals ("bell metal")
about 30% Silver-white, glassy-brittle, polishes like a mirror Mirrors ("speculum metal")

What you need

Item Amount Notes
Copper 900 g for 1 kg of bronze From Copper Smelting smelting, or salvaged
Tin 100 g for 1 kg of bronze Smelted from cassiterite, below
Cassiterite (tin ore) about 200 g per 100 g of tin Cleaned to black grains
Charcoal 3–5 kg per melt See Charcoal
Bellows, tuyere, crucibles As for Copper Smelting
A balance Two pans hung from a stick; see Measurement from Scratch
Moulds Stone, clay or lost-wax, below
Beeswax 50–300 g For lost-wax models; see Beekeeping

Where to find it

Tin is the hard part (the metal itself, and its other uses, are in Tin and Pewter). It is rare, and it is found in only one useful ore: cassiterite (tinstone), tin oxide. Look for it in country with granite — the coarse, speckled pink-white-and-black rock — and especially in the gravels of streams draining granite hills.

Cassiterite is brown to black, glassy to greasy-looking, and astonishingly heavy: a pebble feels like lead in the hand. It is too hard for a steel knife to scratch and its streak is pale. Because it is heavy, it collects with the black sand at the bottom of a gold pan. Pan the streams (see Finding and Identifying Ores). Magnetite in the black sand will jump to a lodestone; cassiterite will not — so you can separate them with a lodestone drawn over the dry concentrate.

Note If no tin can be found, copper that naturally contains a few percent of arsenic makes "arsenical bronze", the alloy of the earliest Bronze Age. It is nearly as good as tin bronze. But it is made by smelting arsenic-bearing ores, which give off deadly fumes (see Dangers). Use it only if you have no other choice, and only in the open air.

Method 1: Smelting tin

  1. Concentrate the ore. Pan the stream gravels until you have mainly black grains. Draw out the magnetite with a lodestone. Pick out light-coloured grains. Your concentrate should be dark brown to black, and so heavy that a cupful of it weighs about four times as much as a cupful of water.
  2. Crush any coarse pebbles to grains of 1–3 mm.
  3. Mix one volume of cassiterite with one volume of charcoal powder.
  4. Smelt in a crucible exactly as in Copper Smelting Method 2: crucible buried in charcoal, blast from above. Cassiterite is harder to reduce than copper ore, so the fire must be hot and strongly smothered: keep the crucible deep under charcoal and hold it at a yellow heat (about 1,100–1,200 °C) for a full hour.
  5. Collect the tin. When cool, break out the contents. Tin forms silvery-white beads and a button at the bottom. Crush the slag and pan it for more beads.
  6. Purify. Melt the beads together in a clay dish at a low red heat (well below what you used to smelt). Skim off the dross and pour the bright liquid tin into a small mould, or onto a flat stone to make thin sheet.

Tip Testing tin. Tin is soft, silvery-white and very heavy. Bend a bar near your ear: pure tin gives a faint crackling noise called the tin cry. A small piece melts easily on the edge of a cooking fire. If it doesn't melt, it is not tin.

Method 2: Alloying

  1. Weigh. Use a balance to weigh 9 parts of copper and 1 part of tin. For your first bronze, 450 g of copper and 50 g of tin is plenty.
  2. Melt the copper first, in a crucible under a layer of charcoal, as in Copper Smelting Method 4. Bring it to a bright orange-yellow heat, until it is a swirling liquid.
  3. Add the tin. Drop the tin in through the charcoal layer. It melts instantly and dissolves into the copper. Stir once with a dry green stick.
  4. Reheat briefly — 2 to 3 minutes of full blast — then skim and pour. Bronze needs to be poured at about 1,100–1,150 °C (orange-yellow), hotter for thin or detailed castings.

Alternative: cementation. You can also add clean cassiterite grains directly to molten copper under a thick layer of charcoal, and keep it hot for 20–30 minutes. Some tin is reduced straight into the copper. It is harder to control how much tin you end up with, but it skips smelting tin separately.

Method 3: Casting

Bronze flows far better than copper, so you can cast more complicated shapes. In every mould, the metal goes in through a funnel-shaped pouring cup (or sprue) and air must be able to get out. Every mould must be bone-dry and preheated.

Open stone moulds — carved into one face of a block of fine sandstone or soapstone — make flat shapes: flat axes, chisels, ingots, sickle blades. See Copper Smelting Method 4.

Two-piece (bivalve) moulds make shapes with two faces, like a spearhead or a socketed axe. Carve matching halves in two stone blocks that sit flat together, with a pouring cup carved at one end. Peg or tie the halves together with cord and seal the joint with clay. For a clay version, press a model (wood or an earlier casting) halfway into a slab of clay, dust it with fine ash so it won't stick, press a second slab on top, separate, remove the model, cut a pouring channel, dry and fire.

Lost-wax casting makes shapes that no two-piece mould can: rings, figures, bells, hollow handles, complicated machine parts.

1 · Wax modelwith sprue andpouring cup 2 · Investfine clay coats,then coarse clay 3 · Melt outcup down; then firethe mould red-hot 4 · Pourinto the hot mould,set in dry sand 5 · Break outsaw off the spruealong the dashes cup fine clay slip wax
Fig. 2 Lost-wax casting, step by step. The wax model is coated in clay, the wax is melted out, and bronze takes its place.
  1. Model in wax. Warm beeswax in your hands (or mix 3 parts beeswax with 1 part pine resin for a firmer wax) and shape the object exactly as you want it in metal. Smooth it with a warm wet finger.
  2. Add a sprue. Stick a rod of wax 1 cm thick to the thickest part of the model and end it in a wax cone 3 cm across: this becomes the pouring cup. For large models, add thinner wax rods from the high points to the outside as air vents.
  3. Invest it. Mix very fine clay with water to a cream (sieve through cloth), with a little finely ground charcoal or dung. Paint it all over the model with a feather or brush. Let it dry; paint two more coats. This fine layer captures the detail.
  4. Build the mould. Pack 1.5–3 cm of coarser clay mixed with sand and chopped straw or dung around it, leaving the end of the pouring cup open. Dry slowly in shade for several days until it is completely dry.
  5. Melt out the wax. Set the mould cup-down on two stones over a gentle fire and catch the running wax in a dish to reuse. Then fire the mould in the embers to a dull red heat (about 600–700 °C) for an hour to burn out the last wax and drive out all moisture.
  6. Pour while the mould is still hot: stand it cup-up in dry sand, and pour bronze in one steady stream until the cup stays full.
  7. Break it out when cool. Saw or chisel off the sprue and vents, then finish with stone files, sand and hammering.

Method 4: Hardening by hammering

Cast bronze is already about twice as hard as cast copper. Cold hammering makes it harder still — the same work hardening you used on copper, but stronger.

  1. Hammer the edge cold on a smooth anvil stone with a smooth hammer, working along the edge in overlapping blows. Thin it by about one-third to a half.
  2. Anneal if it starts to feel springy or shows tiny cracks: heat to dull red (about 600 °C, just visible in shade) and let cool or quench. Then continue hammering.
  3. Finish with hammering, not annealing. The last work on a cutting edge is always cold hammering. Then grind it sharp on sandstone with water.

A well work-hardened 10% bronze edge is roughly four times harder than soft copper. It will cut wood and bone cleanly and can be resharpened many times.

Material Relative hardness (rough) Notes
Annealed copper 1 Bends, dulls fast
Hammered copper 2 Usable for awls and soft materials
Cast 10% bronze 2 Casts beautifully
Hammered 10% bronze 4 Tool edges; compares with unhardened mild steel
Hardened and tempered Steel 10 or more The goal of the iron chapters

How to tell it worked

  • Colour. 10% bronze is golden, warmer than brass and paler than copper. More tin makes it paler and greyer; high-tin bronze is nearly white.
  • Ring. Tap a bronze bar hanging from a cord: it rings clearly. Copper gives a dull clunk.
  • Hardness. A bronze edge should scratch copper easily and hold its edge when you whittle hardwood.
  • Break test. Notch and break a test bar. Good bronze shows a fine-grained, golden break. A grey, coarse break means too much tin; holes mean gas or a wet mould.

Note Troubleshooting. Tin won't come out of the cassiterite → not hot enough, or too much air reaching the crucible. Bury it deeper in charcoal, smaller charcoal, longer at yellow heat. Bronze cracks when hammered → too much tin (over about 13%), or you forgot to anneal. Check your weights. Lost-wax casting incomplete → the mould was too cold or the bronze too cool. Pour straight from the fire into a red-hot mould. Mould burst or spat metal → it was damp. Dry for longer and fire to red heat before pouring.

Dangers

Danger Arsenic and lead. Arsenical copper ores, and arsenic-rich slag, give off a white smoke that smells of garlic and can kill; long exposure causes nerve damage and cancer. Old bronze recipes often add lead to help casting; lead fumes and dust are a slow poison, especially to children. Work in the open, upwind, and never use your melting crucibles for food.

Danger Damp moulds explode. Molten bronze meeting water inside a mould turns it to steam instantly, which can blow metal out of the pouring cup into your face. Every mould must be bone-dry and preheated. Never pour over wet ground.

  • Burns and fire — as in Copper Smelting. Wear leather and wool, plan the path from fire to mould, and keep the quenching water well away.
  • Carbon monoxide — every charcoal furnace makes it. Work in the open.

What this unlocks

Bronze gives you good edge tools and, above all, castings: gear wheels for Gears, bearings for the The Wheel and Axle, valves and cylinders for pumps and the The Steam Engine, and bells. The casting skills here are expanded in Metal Casting. When you are ready for something stronger and cheaper, move on to Iron (the Bloomery).

How it was first done

The earliest true tin bronze known is a piece of foil from Pločnik in Serbia, made around 4,600 BC. Before tin bronze became common, people in the Near East used arsenical copper for over a thousand years. Tin bronze spread across the Near East and Europe from about 3,000 BC, and in China the Shang dynasty (about 1,600–1,050 BC) cast enormous, finely decorated bronze vessels in clay piece-moulds. Because tin is rare, it was traded over thousands of kilometres — from Cornwall, from central Asia, from the mountains of central Europe. A ship that sank off Uluburun, Turkey, about 1,300 BC carried about ten tonnes of copper ingots and one tonne of tin: the recipe for bronze, in a ship's hold.

Source: content/entries/metals/bronze.md