◆ Rebuild

Part 13 · Electricity

The Rechargeable Battery

Two kinds of lead plate in dilute sulfuric acid make a battery you can charge from a generator and use again hundreds of times — Planté's lead-acid cell and Faure's pasted plates. How to make, form, charge, use and look after them, and how to build the nearly indestructible nickel-iron cell of Edison.

Difficulty
●●●●●
Time
An afternoon to build a Planté cell; weeks to form it fully. A few days for a pasted-plate cell once you have red lead
Steps from zero
22 prerequisites →

You need first

The BatteryLeadSulfuric Acid

This unlocks

Lithium BatteriesStoring Energy
The full path from nothing — 22 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Lime
  14. Fermentation
  15. Lye and Potash
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Copper Smelting
  20. Lead
  21. Sulfuric Acid
  22. The Battery
  23. The Rechargeable Battery

Do them roughly in this order. See it on the tech tree →

Why it matters

The batteries in The Battery make electricity by eating zinc, and when the zinc is gone they are finished. A rechargeable battery — also called an accumulator or storage battery — makes no electricity of its own. You pour electricity in from a The Generator, it stores it as a chemical change in its plates, and it gives nearly all of it back later. Then you charge it again, hundreds of times.

That changes what electricity can do:

And it needs no zinc at all — only Lead and Sulfuric Acid, both of which this book shows how to make.

How it works

A lead-acid cell has two sets of plates in dilute sulfuric acid:

  • Positive plates coated with lead dioxide, a dark chocolate-brown powder.
  • Negative plates of spongy lead, soft and grey, full of tiny pores.
−+ Separatorsgrooved wood, glassrods or perforated clay Negative platespongy lead, grey Positive platelead dioxide,chocolate brown Acid level1–2 cm above plates Acidabout 1.25 times asheavy as water whencharged Ribsplates stand clear Sediment space3–5 cm; shed pastefalls here One cell: about 2 volts, whatever its size jar of glass or glazed stoneware
Fig. 1 A lead-acid cell. Positive plates (brown) and negative plates (grey) alternate, kept apart by separators, all fully under the acid. The positive plates are joined to one terminal and the negatives to the other. They stand on ribs above a sediment space where loosened paste can fall without shorting the plates.

Discharging: when current flows, both the lead dioxide and the spongy lead react with the acid and turn into lead sulfate. The acid's sulfate goes into the plates, so the acid gets weaker and lighter.

Charging: push current backwards through the cell from a DC source, and the change runs in reverse: lead sulfate turns back into lead dioxide on the positive plates and spongy lead on the negatives, and the acid gets stronger again. At the end of charging, when there is little sulfate left, the current starts splitting water instead, and both plates bubble — hydrogen at the negatives, oxygen at the positives (Electrolysis).

−+ −+ Dischargegives current; both plates turnto lead sulfate; acid weakens ChargeDC in, + to +; 2.4–2.6 V per cell;acid strengthens; gas at the end Charged Discharged − grey spongy lead | + dark brown acid 1.25–1.28 times water's weight 2.1 V resting hydrometer floats high both plates paler: + light brown acid about 1.12–1.15 1.8 V under load: stop here hydrometer sinks deeper
Fig. 2 Charging and discharging. A charged cell has dark brown positive plates, grey negative plates and strong acid; a discharged one has paler plates and weak acid. The weight of the acid, read with a hydrometer, shows how charged the cell is.

The numbers

Value per cell
Voltage, charged, at rest 2.05–2.15 V
Voltage while giving current about 2.0 V, falling slowly to 1.9 V
Stop discharging at 1.8 V (under load)
Voltage needed to charge 2.2 V at the start, rising to 2.5–2.7 V at the end
Gassing begins at about 2.4 V
Acid, fully charged 1.25–1.28 times as heavy as water
Acid, discharged 1.12–1.15
Ampere-hours returned for each put in 85–90%
Energy returned (watt-hours) 70–80%

The voltage of a cell does not depend on its size — every lead-acid cell gives about 2 V. Its capacity (how many ampere-hours it holds) depends on the amount of active material on its plates. For more voltage, join cells in series: 3 cells for 6 V, 12 for 24 V, 55 for 110 V.

The ampere-hour (Ah) is the measure of capacity: a 50 Ah cell gives 5 A for 10 hours, or about 2.5 A for 20 hours. Drained fast, it gives less: at the 1-hour rate, only about half its 10-hour capacity.

What you need

Item Amount Notes
Lead 3–5 kg per cell of 20–50 Ah Lead, as pure as possible
Sulfuric acid About 1 litre of battery acid per 3 kg of plates Sulfuric Acid: free of iron, nitric acid and salt
Rainwater or distilled water Plenty Distillation; never well water with minerals
Jars One per cell, 2–5 litres Glass or glazed stoneware (Glazes); or wooden boxes lined with pitch
Separators Strips of grooved wood, glass rods, perforated glazed clay Boil wood in water first to remove its acids
Red lead and litharge For pasted plates Made from lead (Lead)
DC supply 2.5–2.7 V per cell, at a tenth of the capacity in amps The Generator with a commutator, or primary cells (The Battery)
Hydrometer One Made below
Meters Voltmeter and ammeter Measuring Electricity

Where to find it

  • Lead comes from galena, the heavy, shiny grey ore with cube-shaped crystals (Lead, Finding and Identifying Ores). For battery grids, antimony — a few per cent, from the grey, needle-crystalled ore stibnite — hardens lead so the plates do not sag; but pure lead works, and pure lead cells hold their charge longer.
  • Litharge and red lead are made by heating lead in air, as described in Lead: litharge is the yellow-orange crust on molten lead, and red lead is litharge roasted gently for hours at about 450–480 °C until it turns scarlet.
  • Sulfuric acid — see Sulfuric Acid. It must not contain iron (which is why rusty vessels are banned near batteries), nitric acid, or salt.
  • For the nickel-iron cell: nickel from green garnierite (Nickel and Cobalt); potash from wood ash (Lye and Potash).

Battery acid

Pour strong acid slowly into about three times its volume of rainwater, stirring, in a glass or stoneware vessel standing in cold water. Let it cool. Then adjust: by weight, a cup that holds 100 g of water should hold about 125 g of finished battery acid (see the table in Sulfuric Acid).

A hydrometer

Seal the end of a glass tube about 12 cm long and 1 cm across into a small bulb (Glass, Laboratory Glassware). Drop lead shot into the bulb until the tube floats upright in rainwater with most of its stem showing. Seal the top. Float it in water and scratch a mark at the water line: 1.00. Float it in acid you have weighed to be 1.25 and mark that. Mark 1.10, 1.15 and 1.20 by making up acids of those weights too. Keep it in a tall glass jar; draw a sample of acid from a cell with a glass tube and your finger over the top, or a rubber bulb if you have Rubber.

Method 1: The Planté cell

This is the simplest storage cell: two sheets of plain lead in acid. The active material grows out of the lead itself by repeated charging, called forming. It is slow and holds less than a pasted cell, but it is very hard to get wrong, and Planté plates last for many years.

Build it

  1. Plates. Cast or hammer lead sheet 2–3 mm thick. Cut plates about 15 × 20 cm, each with a lug 3 cm wide and 8 cm long at one top corner. Make an odd number — say 3 negatives and 2 positives, or 5 and 4. The outer plates are always negative.
  2. Roughen them. The more surface, the more capacity. Score both faces with close parallel grooves 1–2 mm deep using a toothed scraper, or hammer them over a coarse file. Planté found that soaking new plates for a day in nitric acid (Nitric Acid) diluted with an equal volume of water etches them and greatly speeds forming; rinse them thoroughly afterwards.
  3. Assemble. Stand the plates in the jar on two glass or wooden ribs, 3–5 cm above the bottom, alternating negative and positive, about 8–10 mm apart. Put separators between every pair so they can never touch. Lugs of all positives go on one side, negatives on the other.
  4. Join the lugs with a strap of lead. Join lead to lead by melting them together with a hot iron or a small flame (lead burning). Solder and brass corrode in acid fumes; if you must use a copper wire, join it to the lead strap well above the acid and coat the joint with tallow.
  5. Fill with battery acid diluted a little more than usual for forming (about 1.15), to 1–2 cm above the plates.

Form it

Planté formed his cells by charging them, discharging them, then charging them the other way, over and over, so that both sets of plates were attacked and roughened deeper each time.

  1. First charge. Connect the DC supply: + to the plates you have chosen as positive. Charge at a low current — about 0.5 A per dm² of positive plate surface — until both sets of plates bubble freely. The positives turn brown.
  2. Rest and discharge. Let it stand an hour, then discharge it through a resistance (an iron wire coil, or a lamp) until the voltage under load falls to about 1.8 V.
  3. Reverse. Charge it the other way round until it gasses; discharge; reverse again. Make each charge a little longer than the last.
  4. After about ten reversals over a week or two, finish by charging always in the correct direction. Continue cycling — charge fully, discharge to 1.8 V — for some weeks more. The capacity grows with every cycle.
  5. Finish: positives a deep chocolate brown, negatives a light slate grey, both evenly coloured. Replace the forming acid with fresh battery acid at about 1.25.

A plain-sheet Planté cell holds little for its weight: expect a few ampere-hours for a cell of the size above after a month of forming, more as it ages. Deep grooving, or building plates from many thin ribs, multiplies the surface and the capacity.

Method 2: Pasted plates (Faure)

In 1881 Camille Faure found a short cut: spread the plates with lead oxide paste, and one long charge turns it into active material. Pasted plates hold several times as much for their weight as Planté plates. They are less robust: the paste slowly falls out after some hundreds of cycles.

  1. Cast grids. Carve or cut a mould in stone, iron or dry hardwood (Metal Casting): a frame with a lug, filled with a lattice of bars leaving square holes about 1 cm across, the whole plate 4–6 mm thick and about 15 × 20 cm. Cast in lead hardened with 3–5% antimony if you have it.
  2. Positive paste. Mix red lead (or red lead with a third of litharge) with dilute acid (about 1.10) to a stiff, buttery paste, like mortar.
  3. Negative paste. Litharge mixed the same way, with a pinch of lampblack (soot) and a spoonful of fine sawdust per kilogram. These keep the negative material porous; without them it shrinks and hardens after a few dozen cycles.
  4. Paste the grids. Press the paste firmly into the holes with a wooden spatula from both sides, filling them flush. Expect roughly 1 Ah of capacity for every 10–15 g of dry positive paste.
  5. Cure. Keep the pasted plates in a warm, damp place — under wet sacking — for 1–3 days, then let them dry slowly. Curing sets the paste hard so it will not wash out.
  6. Assemble as for the Planté cell, with separators.
  7. Form with one long, gentle charge: fill with acid of about 1.15, and charge at about a twentieth of the expected capacity in amps (2.5 A for a 50 Ah cell) for 24–48 hours, until both sets of plates gas freely and the acid has stopped strengthening for three hourly readings. Discharge once to 1.8 V, recharge fully, and adjust the acid to 1.25–1.28.

Charging and using the battery

Charging

  1. DC only, + to +. Join the supply's positive to the battery's positive. Charging the wrong way round ruins plates. Check with a galvanometer or by which plate bubbles in salt water if you are unsure (The Battery).
  2. Voltage. You need at least 2.5 V per cell, so a supply a little higher than the battery: 3 cells need 7.5–8 V; 12 cells need 30–32 V. Control the current with a resistance in series.
  3. Rate. Charge at about a tenth of the capacity (5 A for a 50 Ah battery). When the cells begin to gas, halve the current.
  4. Full charge is reached when: both plates gas freely ("boiling"); the hydrometer reading has stopped rising for three readings an hour apart; and the voltage, while still charging, has stopped rising at 2.5–2.7 V per cell.
  5. From primary cells: three Daniell cells in series (3.3 V) will slowly charge one lead-acid cell. It works, and is how the first storage cells were charged, but it eats zinc and is only for small cells.
  6. From a dynamo: prevent backflow. If the dynamo slows down or stops while connected, the battery pushes current back through it and drives it as a motor, or burns its windings. Disconnect the battery before the dynamo slows, or fit a cut-out: a relay (The Electromagnet) whose coil is fed by the dynamo and which closes the charging circuit only while the dynamo's voltage is higher than the battery's.

Using it

  • Never discharge below 1.8 V per cell under load, or below about 1.15 on the hydrometer.
  • Never leave it discharged. Recharge within a day. A cell left flat grows hard, white lead sulfate crystals that the current cannot turn back — sulfation — and loses capacity for good.
  • Equalising charge. Once a month, after an ordinary full charge, continue at a quarter of the normal rate for 3–4 more hours. This brings every cell to full charge together.
  • Top up with rainwater or distilled water, never with acid. Water is lost as gas when charging; the acid stays. Add acid only to replace acid that has spilled.
  • Keep it clean and dry. Damp acid film on the tops of cells leaks current between terminals. Wipe with a cloth damp with soda water, then dry.
  • Keep it charged in winter. A charged cell freezes only below about −50 °C; a flat one freezes at about −7 °C and cracks its jar.
  • Standing, a cell slowly loses charge — a few per cent a week, more if the lead contains antimony. Give an idle battery a freshening charge every month.

Method 3: The nickel-iron (Edison) cell

The nickel-iron cell is the toughest battery ever made. It does not mind being overcharged, fully drained, left flat for months, or frozen; Edison cells built around 1910 still work. Its drawbacks: it gives only 1.2 V per cell, returns only about 60% of the energy put in, gives off a lot of hydrogen, and needs nickel, which is scarce. It is worth building only if you have nickel and need a battery that will outlast you.

It is an advanced project. In outline:

  1. Positive material: nickel hydroxide. Dissolve nickel (Nickel and Cobalt tells how to get it from its ores) in dilute sulfuric acid to make green nickel sulfate solution. Stir in caustic soda or caustic potash solution (Lye and Potash, Electrolysis): a pale green sludge of nickel hydroxide settles. Wash it many times in rainwater and dry it. Mix it with fine flakes of graphite (or thin nickel flakes, as Edison did) so that it conducts.
  2. Negative material: fine iron. Precipitate iron hydroxide in the same way from green vitriol (iron sulfate), dry it, heat it to red to make oxide, then heat it again in a closed iron tube with powdered charcoal (or in hydrogen) to reduce part of it to a fine iron powder.
  3. Pockets. Pierce thin sheet steel with hundreds of fine needle holes, fold it into flat pockets or tubes about 1 cm across, pack them hard with each material, and crimp them into steel frames. Nickel-plate the steel if you can (Electroplating).
  4. Electrolyte. A solution of about 21% caustic potash in distilled water. Edison added a little lithium hydroxide, which lengthens life, but it is not essential.
  5. Container. Sheet steel, welded or riveted and sealed. Alkali does not attack iron. Insulate the cans from each other: each can is connected to its plates.
  6. Charge at 1.6–1.8 V per cell; the cell gives about 1.2 V. Five nickel-iron cells do the work of three lead-acid cells.
  7. Care: keep a tight lid with a small vent; air spoils the electrolyte by turning it to carbonate. Replace the electrolyte every few years.

The related nickel-cadmium cell (Jungner, 1899) uses cadmium instead of iron; it works better in the cold but cadmium is rare and poisonous.

How to tell it worked

  • Colour. Charged positives dark chocolate brown; negatives slate grey. Hard white spots on either mean sulfation.
  • Voltage. About 2.1 V per cell at rest after charging, holding above 1.9 V for most of a discharge at the 10-hour rate.
  • Hydrometer rises from about 1.12–1.15 (flat) to 1.25–1.28 (charged), the same in every cell.
  • Capacity test. Discharge a fully charged battery through a fixed resistance, reading the ammeter every half hour, until the voltage reaches 1.8 V per cell. Amps × hours = capacity. It should rise over the first weeks of use, then stay steady for years.
  • Holding charge. After standing a week, a good cell still reads within 0.02–0.03 of its charged hydrometer value.

Note Troubleshooting. One cell reads lower than the rest → it is short-circuited (a plate touching, or sediment piled up to the plates), or it was weaker to begin with. Find the short; give the whole battery an equalising charge. Cell gets hot while charging → charging too fast, or a short circuit inside. Halve the current; check the separators. Paste falling out of pasted plates → charged or discharged too fast, or not cured. Cure longer; charge more gently. Plates warp and buckle → heavy discharge or overheating; also plates of soft pure lead too thin. Use thicker or antimony-hardened grids. White crust, little capacity → sulfation. Dilute the acid to about 1.10 with water, then charge at a very low rate (a fiftieth of capacity) for several days. Readjust the acid when it is charged. Badly sulfated plates cannot be saved. Cell loses its charge in days → impurities (iron, copper, chlorine, nitric acid) in the acid or water. Empty it, rinse with rainwater, refill with pure acid. Nickel-iron cell weak → electrolyte turned to carbonate by air, or level too low. Renew it.

Dangers

Danger Charging batteries give off hydrogen and oxygen — an explosive mixture. A single spark at a terminal can blow the top off a cell and spray acid into your face. Charge in a well-aired room or outdoors, never in a closed box or cupboard. No flames, pipes or lamps nearby. Make and break connections at the charger or switch, never at the battery terminals, and wait half an hour after charging before working on the battery. Wear eye protection.

Danger Short circuits. A lead-acid battery can deliver hundreds of amps. A spanner dropped across its terminals can glow red, weld itself in place and explode a cell. A ring or watch that touches two terminals burns to the bone. Remove metal jewellery, use tools with wooden handles, and cover terminals.

Danger Lead dust poisons. Red lead, litharge and dried paste are fine powders of lead. Breathed or swallowed, they cause lead poisoning: tiredness, stomach cramps, a blue line on the gums, and lasting damage to the brain, especially in children. Mix pastes wet, never sweep dry dust (wet-mop it), wear a damp cloth over the mouth and nose, wash before eating, keep children and food away. See Lead.

  • Acid in the cells burns skin, eyes and clothes. Wash splashes at once with plenty of water; keep a bucket of water with washing soda beside the battery. Always add acid to water, never water to acid (Sulfuric Acid).
  • Caustic potash in nickel-iron cells is as dangerous to the eyes as caustic soda (Lye and Potash).
  • Weight. A battery of large cells weighs hundreds of kilograms. Build a strong rack of acid-proof, tar-painted wood at a working height.
  • High voltage from many cells in series: 50 cells give 100 V, which can kill. Treat a large battery like a dynamo (Wiring and Electrical Safety).

What this unlocks

How it was first done

In 1854 the German physician Wilhelm Sinsteden noticed that lead plates in sulfuric acid, after a current had passed, could give back a current of their own. In 1859 the French physicist Gaston Planté built the first practical rechargeable cell: two long sheets of lead separated by strips of rubber, rolled into a spiral and immersed in dilute sulfuric acid; he showed it to the French Academy of Sciences in 1860 and spent years improving the forming process. Planté's cells could only be charged from primary batteries until the dynamo arrived in the 1870s. In 1881 Camille Faure patented pasted plates, and Ernest Volckmar and John Scudamore Sellon the cast lead grid that held the paste. Henri Tudor of Luxembourg built reliable large Planté-type batteries from the 1880s, used to steady the first town power stations. The Swedish inventor Waldemar Jungner made the nickel-cadmium cell in 1899, and Thomas Edison, hoping to power electric cars, patented the nickel-iron cell in 1901 and sold it from about 1910. Electric cars and delivery vans running on lead-acid batteries were common in cities around 1900–1915, before petrol cars took over.

Source: content/entries/electricity/lead-acid-battery.md