◆ Rebuild

Part 13 · Electricity

Electric Kilns and Furnaces

Wind resistance wire into the walls of a well-insulated box and you have a kiln that fires pottery, enamel and glass with no smoke, no stoking and a temperature you can set to the degree. How to design and build the electric kiln, the laboratory muffle and tube furnaces, and the induction furnace that melts metal from the inside, and how to measure and control their heat.

Difficulty
●●●●●
Time
One to two weeks to build a small electric kiln once you have wire and bricks; a few days for a muffle or tube furnace; months for a working induction furnace
Steps from zero
30 prerequisites →

You need first

Electric Kettles, Irons, Heaters and CookersFirebrick and Refractories

This unlocks

Very-High-Temperature Furnaces
The full path from nothing — 30 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Bricks
  14. Fermentation
  15. The Wheel and Axle
  16. Firebrick and Refractories
  17. Bellows
  18. Gears
  19. Copper Smelting
  20. Iron (the Bloomery)
  21. The Waterwheel
  22. Blacksmithing
  23. Magnets
  24. The Battery
  25. Copper Wire
  26. Electrolysis
  27. Nickel and Cobalt
  28. The Generator
  29. Wiring and Electrical Safety
  30. Electric Kettles, Irons, Heaters and Cookers
  31. Electric Kilns and Furnaces

Do them roughly in this order. See it on the tech tree →

Why it matters

A wood kiln (The Kiln) needs a day of stoking, burns a cartload of fuel and fills the ware with ash and smoke. An electric kiln needs a switch. Its heat is clean, so glazes and enamels stay pure; even, because elements line every wall; and repeatable, so a workshop or laboratory can work to a recipe.

Electric kilns fire Glazes, Stoneware and Porcelain and Enamel on Metal in a shed. A small muffle furnace hardens and tempers tool steel (Alloy and Stainless Steels), assays ores (Gold and Silver) and burns samples to ash for analysis (Identifying Substances). A tube furnace heats things in a stream of hydrogen or nitrogen, which is how you make the copper-oxide and germanium devices of Semiconductors and the Transistor and purify materials for Pure Silicon. The induction furnace melts metal by making it heat itself.

You need a strong supply: a small kiln takes 2–5 kW, as much as two or three electric kettles running for eight hours (Power Lines and Distribution, Wiring and Electrical Safety).

How it works

Heat in, heat out

A furnace gets hotter until it loses heat through its walls as fast as the element supplies it (Electric Kettles, Irons, Heaters and Cookers). So there are only two ways to go hotter: more power or better insulation. A thick, light, porous wall is worth more than extra wire.

As a guide for a small kiln with 7–8 cm walls of insulating brick:

Top temperature Power per litre of chamber
1,000–1,100 °C (earthenware, enamel, glass) 40–50 W
1,200–1,300 °C (stoneware, porcelain) 60–80 W

Smaller kilns need the top of the range, because a small box has more wall for each litre inside.

The wire

The element wire runs 100–150 °C hotter than the chamber, because heat has to flow out of it. So the wire limits how hot the kiln can get.

Wire Wire's own limit Highest useful kiln heat
Nichrome (80% nickel, 20% chromium) about 1,150–1,200 °C about 1,050–1,100 °C: earthenware, enamel, glass
Iron–chromium–aluminium (about 22% chromium, 5–6% aluminium, the rest iron; sold as Kanthal) about 1,400 °C about 1,280 °C: stoneware and porcelain
Platinum (lab furnaces only) 1,500 °C 1,400 °C in tiny furnaces

Nichrome is made as in Nickel and Cobalt. The iron–chromium–aluminium alloy is low-carbon ferrochrome (Alloy and Stainless Steels) and Aluminium melted into soft iron, hot-rolled and drawn warm. It goes brittle after its first firing, so wind and bend it only while new; in return it has a third more resistance per metre and grows a protective skin of alumina.

Watts per square centimetre

The wire's temperature depends on how hard each square centimetre of its surface must work. A coil lying in a groove in a brick wall sheds heat badly, so load it lightly:

  • Kiln coils in grooves, for stoneware: at most 2–2.5 W per cm² of wire surface.
  • For earthenware and enamel: up to 3 W per cm².

A lighter load means a longer life. Elements that run too hot sag, thin and burn out in a few dozen firings.

What you need

Item Notes
Resistance wire Nichrome or iron–chromium–aluminium, 1.3–2.5 mm thick for kilns, 0.5–1 mm for small lab furnaces
Insulating firebrick Light, porous brick that stands 1,250 °C or more; see below
Dense firebrick or kiln shelves Floor, shelves, posts (Firebrick and Refractories)
Fireclay, kaolin, calcined alumina Cements, element-holding tubes, muffles (Finding and Preparing Clay, Alum and Alumina)
Sheet steel and angle iron Outer case, bands, lid frame (Sheet Metal and Rolling)
Heavy cable, fused switch, earth wire Sized for the full current (Wiring and Electrical Safety)
Thermocouple and meter, pyrometric cones Thermocouples and Thermoelectricity, below
Ceramic porcelain bushes To carry the element ends through the wall (Stoneware and Porcelain)

Where to find it

Fireclay lies under coal seams; kaolin is the white clay of rotted granite (Finding and Preparing Clay). Diatomaceous earth is a chalky, very light rock of microscopic plant shells from old lake beds; a dry lump floats briefly on water. Bauxite gives alumina (Aluminium), magnesite gives magnesia, and chromite, heavy and black in green serpentine rock, gives chromium (Alloy and Stainless Steels).

Insulating firebrick

The electric kiln rests on this brick: a third to a half as dense as ordinary firebrick (0.6–0.9 g per cm³), soft enough to carve with a saw blade, and five or six times better at holding heat in.

  1. Mix the clay. Fireclay with some kaolin, tested not to soften below 1,350 °C (Firebrick and Refractories), plus a quarter of its weight of grog (crushed fired brick).
  2. Add burn-out filler. Mix in sawdust sifted through a 2 mm screen, equal in volume to the wet clay. Rice husks or charcoal dust also work. For backing bricks that only see 1,000 °C, use diatomaceous earth bound with a fifth of its weight of clay.
  3. Mould bricks the size of an ordinary firebrick (23 × 11.4 × 6.4 cm) in a wooden mould, pressing firmly. Dry slowly in shade for two weeks.
  4. Fire to at least 50 °C above the brick's working heat. The sawdust burns out, leaving tiny air spaces. Go slowly at 300–500 °C, where it smokes heavily and can flare.
  5. Grind flat. Rub the faces flat on a sheet of sandstone so the bricks fit without mortar gaps.

Good brick does not crumble under a hard thumbnail, and a piece held in a forge flame for two minutes can be picked up by its far end, 5 cm away. Bad brick dusts away (too much filler) or is heavy (too little).

The electric kiln

Lidinsulating brick in anangle-iron frame, hinged Steel jacketearthed; banded tight Insulating firebrick7.5 cm walls Spy hole Coiled elementin grooves 10 cm apart,turns one wire apart Floortwo layers of brick on legs Lid switchcuts both wireswhen lid opens Shelves and postsdense firebrick Terminal boxcold ends on porcelainbushes; covered supply cablevia fused switch Thermocouplein a porcelain sheath,2–3 cm into chamber to meter
Fig. 1 A small top-loading electric kiln, cut away. The walls are insulating firebrick held in a steel jacket. Coiled elements lie in grooves cut in the walls, and their ends pass through porcelain bushes to a terminal box outside. A thermocouple and a spy hole pierce the wall; a switch on the lid cuts the power when it is opened.

The simplest good design is a top-loader: a box of insulating brick on legs, with a hinged lid.

Sizes for a first kiln

Part Size
Chamber 40 × 40 × 40 cm inside (64 litres)
Walls 7.5 cm insulating firebrick (bricks laid flat), plus 2–3 cm of diatomaceous or sawdust brick behind for stoneware
Floor Two layers of insulating brick on a steel plate, raised 15 cm on legs
Lid 9 cm of insulating brick in an angle-iron frame, hinged, with a counterweight
Element grooves 3 or 4 round the walls, 10 cm apart, each about 13 mm wide and 15 mm deep
Power 4 kW for stoneware; 3 kW for earthenware only

Designing the element

Worked example: 4 kW on a 230 V supply.

  1. Resistance = volts² ÷ watts = 230 × 230 ÷ 4,000 = 13.2 Ω. Current = 4,000 ÷ 230 = 17.4 A.
  2. Choose a wire. Iron–chromium–aluminium 2.0 mm thick has about 0.46 Ω per metre. Length = 13.2 ÷ 0.46 = 29 m.
  3. Check loading. Surface = 3.14 × 0.2 cm × 2,900 cm = 1,820 cm². Loading = 4,000 ÷ 1,820 = 2.2 W per cm². Good for stoneware.
  4. With nichrome 2.0 mm (0.35 Ω per metre) you would need 38 m, and could fire only to about 1,100 °C.

On 110 V, use a quarter of the resistance: shorter, thicker elements in parallel. A kiln drawing over about 13 A needs its own circuit, fuse and cable of at least 4 mm² copper.

Winding and fitting

  1. Wind the wire on a steel rod about five to six times the wire's thickness (10–12 mm for 2 mm wire), close-turned on a slowly turning The Lathe, with 30 cm left straight at each end.
  2. Cut the grooves in the wall bricks with a rasp, rounding the corners so the coil does not kink.
  3. Stretch each coil evenly to fill the length of its groove — about two to three times its close-wound length, so the gap between turns is about one wire's thickness.
  4. Lay in. Press the coil into the groove, pinning corners with U-staples of the same wire. Join grooves in series.
  5. Terminals. Pass each end out through a porcelain tube in the wall, twist it double for 8 cm (a cold end), and clamp it on a soapstone or porcelain block in a covered, earthed terminal box.
  6. Case. Wrap the brick in sheet steel, held by bands of strap iron with tightening bolts. Earth the case.
  7. Lid switch. Fit a switch worked by the lid, so that opening the lid cuts both supply wires.

First firing and use

  1. Fire the empty kiln slowly to 1,000 °C over 8–10 hours, lid propped open 2 cm until 600 °C, and hold an hour: this dries the brick and grows the wire's protective skin.
  2. Bisque firing (unglazed clay): 60–100 °C per hour to 600 °C, with the spy hole open; then 150 °C per hour to 950–1,000 °C.
  3. Glaze firing: 150 °C per hour to within 100 °C of the top, then 60 °C per hour, and hold 10–15 minutes.
  4. Cool with the lid shut until below 200 °C. Never open above 300 °C.

Control the rate with a three-heat switch as on an electric cooker (Electric Kettles, Irons, Heaters and Cookers) or an energy regulator (Thermostats and Automatic Control).

The muffle furnace

A muffle is a closed box that keeps the work away from the heat source. Here the wire is wound outside a thin ceramic box, out of reach of hands and of anything that spits or smokes inside.

1 Muffle furnace (end view)2 Tube furnace (lengthwise) Mufflethin clay box steel case Insulating brick7–10 cm kaolin–alumina cement over the winding Wirewound outsidethe muffle Worknever touches the wire Closer turnsat the ends of thewinding Closer turnsends losemost heat stopper,gas in insulation Boat with work bubbler showsgas flowing temperature along the tubeeven hot zone
Fig. 2 Left: a laboratory muffle furnace in cross-section. The wire is wound round the outside of a thin clay muffle and buried in cement, with insulating brick and a steel case outside. Right: a tube furnace. The wire is wound more closely near the ends of the tube, which lose more heat, so the middle third is evenly hot; gas flows through the tube past the work.
  1. The muffle. Make a box of fireclay and kaolin (half and half) with grog, open at one end, walls 6–8 mm thick, about 10 cm wide, 8 cm high and 20 cm deep inside. Score spiral grooves round the outside, 6–8 mm apart, and fire it to 1,250 °C.
  2. Wind. For 1,200 W on 230 V you need 44 Ω: about 20 m of 0.8 mm nichrome, wound first into a small coil on a 4 mm rod, then laid in the grooves, closer near the open end.
  3. Bury the winding in a cement of kaolin and calcined alumina, wetted with a little water glass (Water Glass (Sodium Silicate)), 5 mm thick. Dry slowly.
  4. Insulate with 7–10 cm of insulating brick in a steel case, with a brick door, terminals, earth and door switch as for the kiln.

It reaches 1,000–1,050 °C in about an hour. Use it for hardening tools, enamel tests, fusing glass, ashing samples and copper-oxide rectifiers (Semiconductors and the Transistor).

The tube furnace

When work must be heated in a gas other than air (hydrogen to stop oxidising, nitrogen to stay inert), put it in a wound tube.

  1. The tube. Porcelain, or fused quartz (Fused Quartz and Halogen Lamps) for clean work, both to about 1,100 °C; alumina for hotter. Bore 3–5 cm, length 50–70 cm.
  2. Wind the centre 30–40 cm with 0.6–1.0 mm wire, held in a thin coat of kaolin cement. Use a closer pitch at the two ends of the winding, about twice as many turns per centimetre for the last 5 cm, so the middle third of the tube is evenly hot.
  3. Insulate with a cylinder of insulating brick or diatomaceous earth 8–10 cm thick, in a sheet-steel jacket.
  4. Power: 600–1,000 W reaches 1,000 °C.
  5. Ends. Cork or rubber stoppers with glass tubes; gas leaves through a bubbler of oil or water, so you can see it flowing.

Danger Hydrogen in a hot tube explodes if air is mixed with it. Flush with nitrogen, or with at least ten tube-volumes of hydrogen, before heating. Test a test-tube of the outgoing gas well away: a quiet burn means pure hydrogen, a squeaky pop means air remains. Burn the exhaust in a small flame, and let the tube cool with gas still flowing (Hydrogen, Oxygen and Gases).

The induction furnace

How it works

Alternating current in a coil makes a magnetic field that swings back and forth inside it. A piece of metal inside acts like a The Transformer secondary of one shorted turn: large eddy currents swirl round in it and heat it. The metal heats itself.

The currents crowd into the outside skin of the metal. How deep they reach (the skin depth) shrinks as the frequency rises:

Frequency Skin depth in red-hot steel Good for
50 Hz (mains) about 7–8 cm Large melts of a tonne or more; channel furnaces
1,000 Hz about 1.7 cm Melts of 50 kg to several tonnes
10,000 Hz about 0.5 cm Melts of 1–50 kg; surface hardening
200,000 Hz and up 1 mm or less Small parts, brazing, hardening skins

Heating works well when the metal is at least three to four skin depths across, so small melts need high frequency.

1 Coreless furnace (section)2 Channel furnace cooling water in water out Melteddy currentsheat and stir it Rammedliningmagnesia, aluminaor quartz sand Coilcopper tube,water inside slate orbrick base Capacitor banksupplies thecoil's magnetisingcurrent AC supply500–3,000 Hz Pot Loopof moltenmetal: oneshorted turn Ironcore Primary coilon 50 Hz mains
Fig. 3 The coreless induction furnace. A water-cooled coil of copper tube surrounds a crucible of rammed refractory. Alternating current in the coil drives eddy currents round inside the metal charge, which heat it and stir the melt. A bank of capacitors across the coil supplies most of its magnetising current. Right: a small channel furnace, where a loop of molten metal is the single-turn secondary of a mains transformer.

The coreless furnace

  1. The coil. Copper tube 8–15 mm across (Metal Pipes and Tubes), 8–20 turns, 3–5 mm apart, held between slate or hardwood bars. Water flows through the tube; without it the coil melts in a minute.
  2. The crucible. Ram dry magnesia (for steel) or quartz sand with 1–2% boric acid (for iron and brass), 2–4 cm thick, round a steel former, with mica against the coil. The first melt fuses the face and swallows the former. Small melts can use a clay–graphite crucible (Firebrick and Refractories).
  3. Capacitors. The coil draws a great deal of current that only builds the field. Capacitors across it supply that current; tune them until the line current is smallest (Resistors, Capacitors and Coils).
  4. The supply: a many-pole motor-alternator giving 500–3,000 Hz (The Generator), the industrial standard for fifty years; or a vacuum-tube oscillator (Amplifiers and Oscillators) of 1–20 kW at 100–500 kHz for small melts. The first furnaces used noisy spark-gap oscillators.
  5. Power. Melting steel takes about 0.6–0.7 kWh per kg in a good large furnace, and roughly twice that in a small one, which loses more heat. A 10 kg crucible of steel needs a 20–30 kW supply for half an hour.

The currents also stir the melt, and no fuel gas touches it, so the metal is clean and even.

The channel furnace

With only mains AC and a strong The Transformer, build a channel furnace. Below the pot, a loop-shaped channel in the refractory runs round one leg of the transformer's iron core. Filled with molten metal, the loop is the secondary: one shorted turn, and its heat rises into the pot. The catch: the loop must always stay full. Start it with metal melted elsewhere and never pour the pot empty. If the channel freezes, the furnace is dead until relined. Such furnaces run for weeks melting brass, zinc and cast iron.

The induction heater

A few turns of water-cooled tube shaped to the job, fed at 100–500 kHz, heat a gear tooth or shaft to red in seconds for surface hardening, braze joints with no flame (Soldering and Brazing), and heat the electrodes inside a The Vacuum Tube through the glass while it is on the pump.

Measuring and controlling the heat

Thermocouples

Iron–constantan (Thermocouples and Thermoelectricity) only reaches about 750 °C. For kilns use:

  • Nickel-chromium against nickel-aluminium: 90% nickel with 10% chromium, against about 95% nickel with 2% each of aluminium and manganese. About 41 mV at 1,000 °C and 49 mV at 1,200 °C; good to 1,200 °C.
  • Platinum against platinum–rhodium (10% rhodium): costly and weak (about 9.6 mV at 1,000 °C), but stable to 1,500 °C for years.

Thread the wires through two-hole porcelain tubes inside a closed porcelain sheath, its tip 2–3 cm into the chamber. Calibrate as in Thermocouples and Thermoelectricity.

Cones

A thermocouple tells the air's temperature; pyrometric cones tell what the ware has felt. They are slender pyramids of clay and flux that bend over at a set heat-work. Make a series by stepping the flux in your glaze materials (Glazes, Pyrometric Cones and Kiln Temperature) and calibrate them against the thermocouple. Set three in view of the spy hole, one below, one at and one above the target; when the target cone's tip bends level with its base, the firing is done. A kiln sitter uses a bending cone to trip the power (Thermostats and Automatic Control).

Controllers

The thermocouple controller of Thermostats and Automatic Control switches a contactor (Motor Starters, Contactors and Protection). Keep a firing log: time, switch setting and reading every half hour. After three or four logged firings you can repeat any firing to within a cone.

How to tell it worked

  • The case stays below about 70 °C at full heat: you can touch it for a second.
  • The current matches the design within 5% (Measuring Electricity).
  • Even heat: cones placed top, middle and bottom all bend in the same firing, within one cone of each other.
  • Rate: an empty 64-litre kiln of the design above reaches 1,000 °C in about 4–5 hours at full power.

Note Troubleshooting. Kiln will not reach top heat → walls too thin or cracked, lid gap, low supply voltage under load, or aged elements (replace when resistance has risen 10%). Element burns out at one spot → turns touching, a kink, a glaze drip or a loose terminal. Top fires cooler than bottom → put more wire (or closer turns) in the top groove; most heat escapes through the lid. Tube cracks → heated or cooled too fast, or cold gas striking the hot section. Keep below 300 °C per hour. Induction coil overheats or arcs → water flow too low or a turn touching another. Fit a flow switch that cuts the power if water stops. Induction melt heats slowly → frequency too low for the size of the charge, or capacitors out of tune.

Dangers

Danger Bare elements are live. Kiln wire runs at full mains voltage, uncovered. Never reach in or touch an element with a tool unless the main switch is off. Fit a lid switch that cuts both wires, earth the case, and keep children away.

Danger Water and molten metal. In an induction furnace, cooling water runs centimetres from molten steel. If metal breaks through the lining to the coil, steam throws it out violently. Inspect the lining before every melt and never charge damp scrap (Metal Casting).

Warning Induction fields heat rings and watches near the coil and can upset a heart pacemaker.

  • Fumes. Firings give off sulfur, fluorine, lead fumes and carbon monoxide. Vent the room; never fire where people sleep.
  • Burns and fire. Wear leather gloves; stand kilns 50 cm from walls on brick or stone.
  • Capacitor banks hold a deadly charge after switch-off. Bleed and short them before touching.

What this unlocks

How it was first done

Electric heating waited for a wire that would not burn. In 1906 the American Albert Marsh patented nickel–chromium alloys, and nichrome-wound laboratory furnaces were standard by the 1910s, measured with Henri Le Chatelier's platinum thermocouple and Hermann Seger's cones, both of 1886. Electric pottery kilns spread in the 1920s and 1930s, and in 1931 the Swede Hans von Kantzow introduced Kanthal, which raised them to stoneware heat.

Induction melting was proposed in the 1880s, probably first by Sebastian de Ferranti. F. A. Kjellin ran the first practical channel furnace at Gysinge, Sweden, in 1900, and James Wyatt's Ajax furnace made it the standard for brass from 1916. In the same years Edwin Northrup at Princeton built the first high-frequency coreless furnaces, fed by spark gaps; by the 1930s motor-alternators and tube oscillators had made induction melting and hardening ordinary industrial tools.