◆ Rebuild

Part 8 · Chemistry

Pigments, Paints and Varnish

Dig coloured earths, burn bones and twigs for black, slake lime for white, and grind them fine. Bind the powder with egg, milk curd, gum or linseed oil to make paint that protects wood and walls and keeps records and pictures — then seal it with varnish made from resin.

Difficulty
●●●●●
Time
An afternoon to grind and wash a pigment; minutes to mix most paints; a day to cook oil varnish; paint dries in hours (casein, tempera) to days (oil)
Steps from zero
9 prerequisites →

You need first

Oils and PressingCharcoalLime

This unlocks

Prussian Blue and the PrussiatesLithography and Offset Printing
The full path from nothing — 9 steps before this one
  1. Stone Tools
  2. Fire
  3. Finding and Preparing Clay
  4. Simple Machines
  5. Charcoal
  6. The Kiln
  7. Farming from Seed
  8. Lime
  9. Oils and Pressing
  10. Pigments, Paints and Varnish

Do them roughly in this order. See it on the tech tree →

Why it matters

Paint is a skin you put on things. On wood it keeps out rain and sun, so a painted door, wagon, boat or window frame lasts decades instead of years. On a wall it brightens a room, seals dust and, with lime, kills germs. On a sign, a map, a medicine jar or a warning post it carries information. And on a cave wall, people have used it for at least 40,000 years to say who they were.

Paint is also cheap and forgiving. The raw materials — coloured earth, soot, chalk, lime, oil, milk, eggs — are among the commonest things in this book, and you can make a usable paint the first afternoon you try.

This chapter covers pigments (coloured powders), the binders that glue them down, and varnishes that seal and shine. The same skills make the black of Ink, the glazes of Pottery (Glazes), and the coloured coatings for Roofs, boats, Furniture and Maps and Mapmaking.

How it works

Every paint has two parts:

  1. Pigment — a coloured powder that does not dissolve. It is just very fine grains of coloured mineral, carbon or other solid. (A dye, which dissolves, colours by soaking in — see Dyes and Mordants.)
  2. Binder — a liquid that wets the grains and then sets into a solid film, gluing them to each other and to the surface. Different binders set in different ways:
    • By drying — water evaporates and leaves a glue behind: gum (watercolour), animal glue (distemper), egg yolk (tempera), milk curd (casein).
    • By taking oxygen from the air — drying oils such as linseed, walnut and poppy slowly harden into a tough, flexible skin (oil paint). See Oils and Pressing.
    • By taking carbon dioxide from the air — lime turns back into limestone and locks the colour in (whitewash and fresco). See Lime.

A third, optional part is a thinner — water for water paints, turpentine (Ether, Acetone and Solvents, Tar, Pitch and Glue) for oil — that makes paint flow and evaporates away.

Fineness matters. Colour depends on grain size. Most pigments look richer and cover better the finer you grind them — but a few crystalline minerals, like malachite and azurite, go pale and washed-out if ground too fine. The proportion of binder matters. Too little and the paint rubs off as powder; too much and it is glossy, weak in colour, and may crack or wrinkle.

Too little bindergrains loose: rubs off as dust Just rightevery grain wrapped and glued Too much binderweak colour, glossy, cracks Binder filmoil, egg, gum, caseinPigment grainochre, carbon, chalkSurfacewood, plaster, paper
Fig. 1 What paint is. Fine grains of pigment held in a film of binder. Too little binder leaves loose, dusty grains; too much makes a weak, glossy, cracking film.

What you need

Item Notes
Coloured earths, chalk, lime, charcoal, bones See "Where to find it"
Mortar and pestle Stone or hard-fired stoneware, for crushing
Grinding slab and muller A flat slab of hard, fine-grained stone (granite, basalt, marble, quartzite) about 30–40 cm square, and a hand-sized stone with one flat, smooth face. Grind the two together with wet sand for an hour to make them match. See Abrasives and Grinding Stones
Buckets or pots Three or four, for washing pigments
Palette knife A thin, flexible blade of wood, horn or Steel
Binders Gum arabic, eggs, skimmed milk, slaked lime, linseed oil (see table below)
Brushes Hog bristle, horse hair or squirrel tail bound to a stick, or chewed reed and twig ends. See Brooms, Brushes and Combs
Jars with lids For storing pigments and paints

Where to find it

  • Ochres — soft, earthy iron-oxide clays: yellow ochre (yellow-brown, rusty), red ochre (brick to blood red), brown umber (dark chocolate brown, contains manganese) and sienna (warm yellow-brown). Look in road cuttings, stream banks, eroded gullies, old iron workings, the weathered tops of iron ore beds (gossans — see Finding and Identifying Ores) and the red and yellow bands in sandstone country. A good ochre stains your fingers when rubbed, feels smooth and soapy, not gritty, between the teeth (spit it out), and leaves a strong streak on a white stone.
  • Bog iron (Iron (the Bloomery)) and the orange slime of iron springs dry to yellow ochre.
  • Green earth — dull grey-green clay (glauconite, celadonite), found in some sea-sands and in cavities in volcanic rock.
  • White: chalk (soft white rock, fizzes in vinegar), white kaolin clay (Stoneware and Porcelain), slaked lime (Lime), gypsum (Gypsum and Plaster of Paris), burnt white bone.
  • Black: soot from lamps (see Ink), Charcoal, charred bones, charred vine or willow twigs, and soft black manganese ores (wad, pyrolusite — sooty black, stain the fingers, often in crusts on rock; see Finding and Identifying Ores).
  • Blue and green: azurite (deep blue) and malachite (banded bright green) in the weathered tops of copper deposits (Copper Smelting). They are scarce; Egyptian blue (below) is made from common materials, and later chemistry gives the strong, cheap Prussian Blue and the Prussiates.
  • Binders: eggs and milk from your animals (Keeping Animals), linseed oil (Oils and Pressing), gum arabic or cherry gum (Ink), pine resin (Tar, Pitch and Glue), lac from lac insects in South and Southeast Asia, honey (Beekeeping), flour (Grain, Flour and Bread).

Making pigments

Earth pigments: crush, wash and settle

Raw ochre is full of sand. Washing it out — levigation — is the single most important skill in pigment-making.

1. Stir1 part crushed earthto 5 parts water 2. Wait 30–60 secondssand and grit sink fast 3. Pour offthe cloudy water 4. Settle overnightpour off clear water,dry the fine sludge Grit stayswash it 2–3 more times Muddy colourinto a clean pot Clear water Pigmenta fine layer
Fig. 2 Washing a pigment. Stir crushed earth into water, wait for the sand to sink, and pour the coloured, cloudy water into a second pot. The fine pigment settles there overnight.
  1. Dry and crush the ochre in a mortar to a coarse powder. Pick out roots and stones.
  2. Stir it into a bucket of water — about one part ochre to five parts water — until every lump has broken up.
  3. Wait 30–60 seconds. Sand and grit sink to the bottom.
  4. Pour off the coloured, muddy water into a second bucket, leaving the grit behind. Repeat steps 2–4 with the grit two or three times to recover more colour.
  5. Settle overnight. The fine pigment sinks into a smooth layer. Pour off the clear water above it.
  6. Dry the sludge on a clay plate in the sun, and crush the dry cake to powder.

For extra-fine pigment, do it in stages: what settles in the second bucket after 5 minutes is medium; what is still suspended after 5 minutes, poured into a third bucket and left overnight, is the finest.

Burnt colours

Heating changes ochre. Yellow ochre heated to a dull red heat (roughly 400–700 °C) turns red, as the yellow iron oxide loses its water and becomes red iron oxide. Raw sienna becomes burnt sienna (warm red-brown); raw umber becomes burnt umber (rich dark brown).

Put the powder in a clay pot or on a sherd in hot embers or a The Kiln for 30–60 minutes. Take a pinch out every 10 minutes, let it cool, and compare. Stop when you have the colour you want. This doubles your range from a single pit of yellow earth.

Blacks

  • Lampblack — the finest, bluish black. See Ink and Lampblack and Carbon Black.
  • Vine or twig black — pack dry vine prunings or thin willow twigs in a clay pot, seal the lid with clay, and heat it in a fire until smoke stops leaking (about an hour), as for Charcoal. Grind fine. A soft, bluish black.
  • Bone black — pack clean, broken bones in a sealed clay pot and heat to red for 2–3 hours. They turn deep black. Ground fine, this is the warmest, densest black ("ivory black"). In an open fire, bones burn white instead — bone white, a good white for tempera and for priming.

Whites

  • Chalk — washed as for ochre. Excellent in glue, egg and casein paints; nearly transparent in oil.
  • Lime white — well-aged lime putty (Lime), used in whitewash and fresco.
  • Avoid lead white (see Dangers).

Egyptian blue: a blue from sand

Natural blue minerals are rare. About 4,500 years ago Egyptian craftsmen learned to make a fine, permanent blue from sand, lime and copper — the first synthetic pigment.

  1. Mix by weight: 4–5 parts clean quartz sand (Glass), 2 parts crushed chalk or limestone, 2 parts crushed malachite (or copper scale or bronze filings — see Copper Smelting), and ½ part wood ash or natron as a flux. Grind together finely and moisten into balls.
  2. Fire in a covered clay crucible in a The Kiln at 850–1,000 °C — a bright cherry-red to orange heat — for 10–24 hours. Too cool and it stays grey-green; much hotter than 1,050 °C and the blue breaks down into green glass.
  3. Cool, crush, and fire again for a deeper colour. Then grind — coarse for a deep blue, fine for a pale blue.

Expect several failed batches before you get a strong blue; small changes of heat matter.

The binders

Paint Binder Use it for Sets in Water-resistant?
Watercolour, gouache Gum arabic Maps, books, signs on paper Minutes No
Distemper Hide glue (Glues and Adhesives) Indoor walls and ceilings Hours No
Egg tempera Egg yolk Panels, furniture, fine work Minutes; hardens over months Fairly, once old
Casein ("milk paint") Milk curd + lime Walls, furniture, barns, toys Hours Yes, once cured
Limewash Slaked lime Walls, outbuildings, disinfecting 1–2 days; hardens over weeks Yes, but wears
Oil paint Linseed oil Outdoor wood, iron, boats, art 2–7 days to touch Yes

Gum paint (watercolour)

Dissolve 1 part gum arabic in 2 parts hot water overnight. Add a few drops of honey per spoonful, which keeps the paint from cracking. Grind pigment on the slab with a little of this syrup until smooth: roughly equal volumes of pigment and gum syrup. Thick, with chalk added, it is opaque "gouache". Dry it in shells or small pots; wet it with a brush to use.

Egg tempera

  1. Crack an egg and separate the yolk. Roll the yolk on your palm, dry it with a cloth, pinch the skin and let the yolk drain into a cup; discard the skin.
  2. Add about the same volume of water and stir.
  3. Grind pigment to a stiff paste with water on the slab. Mix paste and yolk medium roughly 1 : 1 on the palette as you paint.
  4. Apply in thin layers. It dries in minutes. Test: a stroke dried for a day should not rub off with a damp finger.

Tempera cracks on anything that flexes. Use it on rigid wooden panels primed with gesso — chalk or gypsum stirred into warm hide glue, brushed on in 6–10 thin coats and scraped smooth.

Casein paint (milk paint)

  1. Let skimmed milk sour and curdle (a day or two in a warm place), or add vinegar until curds form. Heat gently to 40 °C to firm the curds.
  2. Strain through cloth and wash the curd several times in clean water to remove the whey and fat. Squeeze it dry. A litre of skim milk gives about 100–150 g of wet curd.
  3. Stir in lime putty — about 1 part lime putty to 5 parts curd by volume. Keep stirring for 5–10 minutes. The lumpy curd turns smooth, glossy and runny as the lime dissolves it. This is the binder.
  4. Thin with water to the thickness of cream, and stir in pigment that has been soaked in a little water to a paste. Use earths, chalk, lime, carbon and bone black — lime destroys many plant colours.
  5. Use it the same day; it goes off by the next.

On bare wood or plaster it dries flat and velvety within hours, and becomes water-resistant over a week or two. Rub with a cloth dipped in linseed oil for a hard-wearing finish.

Limewash

Thin lime putty with water to skimmed-milk thickness and brush on in several thin coats; full details are in Lime. For colour, add lime-fast pigments — ochres, umbers, burnt colours, charcoal — up to about one part pigment to ten parts lime by volume; stronger than that, it rubs off. A cup of skimmed milk or a handful of salt per bucket makes it harder-wearing.

Linseed oil paint

  1. Use cold-pressed linseed oil (Oils and Pressing), ideally aged a few months and allowed to settle, or thickened in the sun: spread it 1–2 cm deep in a shallow glass or glazed dish, cover loosely against dust, and stand it in the sun for 2–4 weeks until it is like honey.
  2. Put a heap of pigment on the slab, make a well in it, and add oil a little at a time, working it in with the palette knife, then grinding with the muller in small circles. Use the least oil that makes a smooth, stiff, buttery paste. Earths take roughly one part oil to two or three parts pigment by weight; carbon black takes about equal weights and dries very slowly.
  3. Grind each spoonful for 5–10 minutes until there is no grit between your teeth or under the knife.
  4. Thin for brushing with a little more oil, or with turpentine.
  5. Brush out thin. Two or three thin coats, a few days apart, last far longer than one thick coat, which wrinkles and stays soft underneath.

Raw linseed oil paint takes 3–7 days to be dry to the touch. To speed it, use sun-thickened oil, or add a spoonful of raw umber per cup of paint: the manganese in umber acts as a drier. Old recipes used lead compounds for this — do not.

Falu red: cheap paint for barns and houses

The red cottages of Sweden are painted with a cooked flour-and-iron paint that is cheaper than oil paint and lasts 10–15 years on rough-sawn wood:

  1. Boil 10 litres of water in an iron or copper pot.
  2. Whisk 1.5 kg of rye flour into a little cold water, then into the boiling pot. Simmer 15–20 minutes, stirring, until it thickens.
  3. Stir in 0.5 kg of green vitriol (Sulfuric Acid), then 2–2.5 kg of red ochre or burnt yellow ochre, a little at a time.
  4. Stir in 1 litre of linseed oil. Simmer 10 more minutes.
  5. Brush on warm, onto unplaned wood. Two coats.

It dries to a matt, rich red within a day. It is permeable, so wood under it does not rot.

Varnish and lacquer

A varnish is a clear, hard coat: it protects paint and wood and makes colours deep and glossy. It is a resin either cooked into oil or dissolved in a spirit.

Spirit varnish (shellac)

Dissolve 200–250 g of lac flakes (or clear pine rosin, for a softer, cheaper varnish) in 1 litre of strong alcohol — at least 90%, the strongest you can distil. Shake daily for 2–3 days until dissolved. Strain through cloth. Brush or rub on in many thin coats; each dries in 15–30 minutes. It is the classic finish for furniture and the best quick seal for knots in wood before painting. It is spoiled by water and alcohol spills.

Oil varnish

  1. Outdoors, in an iron or clay pot filled no more than one third, melt 1 part rosin (or the harder resins amber or copal, if you can get them).
  2. Separately warm 2–3 parts linseed oil until very hot, hotter than for frying (roughly 200–250 °C — a scrap of bread dropped in browns within a second or two). Do not let it smoke heavily: near this heat its vapour can catch fire.
  3. Pour the hot oil slowly into the melted resin, stirring. Cook gently, testing a drop on cold glass, until a drop pulls a thread between finger and thumb. Take it off the fire.
  4. When it has cooled well below smoking, thin with turpentine to brushing consistency.

Oil varnish is tougher and more water-resistant than shellac, and is the varnish for boats, carriages and outdoor work. It dries in a day or two.

Lacquer

True lacquer is the sap of the Asian lacquer tree (Toxicodendron vernicifluum), tapped like rubber from cuts in the bark in East Asia. It does not dry in dry air: it hardens in warm, humid air (about 20–30 °C and 70–85% humidity), so Japanese craftsmen cure it in damp wooden cupboards. Dozens of thin coats, each polished, make an almost indestructible, glossy surface. Elsewhere, "lacquer" means many thin coats of shellac, rubbed back and polished.

How to tell it worked

  • Rub test: when dry, rub firmly with a finger, then a damp cloth. Good paint does not come off (except gum paint, which should only smear when wet). Powder on your finger means too little binder.
  • Bend test (oil paint and varnish): paint a strip of leather or thin wood, let it dry a week, and bend it. It should flex without cracking.
  • Cover: a good paint hides what is under it in two coats.
  • Grind: no grit or streaks of unmixed colour under the knife.
  • Weather: put painted test boards out in sun and rain for a season before committing a whole house.

Note Troubleshooting. Paint dusts off → too little binder. Add more gum, egg, casein or oil. Cracks like a dry riverbed → too much binder (gum, glue) or a thick coat on a soft base. Thin coats; less binder. Oil paint wrinkles and stays soft → coat too thick, too much oil, or a non-drying oil (olive, rapeseed). Use linseed; brush out thin. Oil paint never dries → wrong oil, or oil has gone rancid. Test your oil alone on glass first: it should be tacky in 2–3 days and dry in a week. Casein paint peels off → curd not washed, or not enough lime, or painted over grease or old oil paint. Varnish turns white and cloudy → water in the alcohol or the resin, or damp weather. Warm the room; use stronger spirit. Ochre colour weak and sandy → not washed. Levigate it.

Dangers

Danger Hot oil and resin fires. Cooking oil varnish is one of the most dangerous jobs in this book: the oil can burst into flame, and water thrown on it explodes it outwards. Work outdoors, far from buildings, with a tight-fitting lid and a bucket of dry sand within reach. If it catches, cover it and walk away; do not lift the lid for an hour. Never add turpentine or alcohol near flame.

Danger Oily rags set themselves on fire. Cloths soaked in linseed oil or oil paint heat up as they dry and can burst into flame hours later. Spread them flat outdoors to dry, or keep them in a closed pot of water.

Warning Poisonous pigments. Many beautiful historic colours are deadly and are best left alone: lead white and red lead (lead poisoning — see Lead), vermilion (cinnabar, mercury — Mercury), orpiment and realgar (arsenic yellows and oranges), green copper-arsenic paints, and verdigris (copper). Painters' "colic" and madness came from these. Earths, carbon, chalk, lime, bone and Egyptian blue are safe.

  • Dust. Grinding dry pigment, even safe ones, damages lungs over years. Grind wet; wipe surfaces with a damp cloth, do not sweep.
  • Lime in casein and limewash burns eyes. Shield your eyes; rinse splashes for 15–20 minutes. See Lime.
  • Lacquer sap is a close relative of poison ivy: touching wet sap causes severe, blistering rashes. Work in gloves and long sleeves; the cured lacquer is harmless.
  • Turpentine and alcohol vapours are flammable and intoxicating. Ventilate.

What this unlocks

Paint protects every wooden thing you build — houses, Wagons and Carriages, boats, Furniture, barrels — and rust-proofs iron (Corrosion and Its Prevention). Pigments colour Glazes and Ink. Clear varnishes insulate Copper Wire and electromagnet windings (The Electromagnet). Colour on paper gives Maps and Mapmaking, illustrated books (Bookbinding) and drawings for teaching (Teaching and Schools). The chemistry of dissolving resins leads to Ether, Acetone and Solvents and Early Plastics.

How it was first done

People were grinding red ochre more than 100,000 years ago: at Blombos Cave in South Africa, an ochre-mixing kit in two abalone shells is about 100,000 years old. The painted caves of Indonesia (Sulawesi, over 40,000 years) and Europe (Chauvet, about 36,000 years; Lascaux, about 17,000 years) used ochre, charcoal and manganese black. Egyptian blue appears around 2600 BC. Egg tempera was the standard panel paint of medieval Europe, and the monk Theophilus described linseed oil paint in the early 12th century; the Flemish painters of the 1400s, such as Jan van Eyck, perfected it. Lacquer was used in China by the Neolithic period, about 7,000 years ago. Falu red paint, from the waste of the great copper mine at Falun in Sweden, spread across Scandinavian farmhouses from the 1700s.

Source: content/entries/chemistry/pigments-and-paints.md