Part 5 · Cloth and Clothing
Silk
Plant mulberry trees, rear silkworms on their leaves for a month, and reel the single long filament off each cocoon in hot water. Silk is the strongest natural fibre for its weight — for fine thread, sutures, wire insulation, sieves, balloons and parachutes.
- Difficulty
- ●●●●●
- Time
- 3–5 years for mulberry trees to give enough leaves; about 6–7 weeks from hatching to reeled silk each season
- Steps from zero
- 2 prerequisites →
You need first
Farming from SeedThe full path from nothing — 2 steps before this one
Do them roughly in this order. See it on the tech tree →
Why it matters
Silk is unlike any other natural fibre. Each cocoon is wound from one continuous filament hundreds of metres long, so silk thread needs no spinning in the usual sense — you unwind it. It is smooth, glossy, very fine and, for its weight, stronger than any other natural fibre. That makes it the material for:
- Fine thread and sewing silk (Sewing, Needles and Thread) and surgical sutures (Basic Surgery, Wound Care and Antiseptics).
- Fishing lines and fine strong cord (Fishing).
- Electrical insulation: silk-covered wire was used in coils and instruments for a century (Copper Wire, The Electromagnet); a single filament hangs compass needles and delicate instruments without twisting (The Compass).
- Sieve and bolting cloth — finely woven silk sifts flour (Grain, Flour and Bread) and fine powders.
- Balloon and parachute cloth — light, strong and, when varnished, gas-tight. The first hydrogen balloon (1783) was rubber-coated silk (Balloons); parachutes were silk until nylon replaced it (Rayon and Nylon).
- Cloth that is light, warm in winter, cool in summer, and beautiful, which for two thousand years made silk one of the most valuable trade goods on earth (Money, Trade and Record-keeping).
Silk is also a demanding craft. It needs years of tree-growing, careful daily work, warmth and cleanliness. Treat it as a project for a settled community, not a first-year survival task.
How it works
The domestic silkworm (Bombyx mori) is the caterpillar of a moth that no longer exists in the wild. After about 5,000 years of breeding it is fat, pale and helpless: the caterpillars do not wander off, and the adult moths cannot fly. It eats almost nothing but mulberry leaves.
- Egg. Tiny (about 1 mm), laid in hundreds on paper or cloth. Most breeds lay eggs that must pass a winter's cold before they will hatch in spring.
- Caterpillar (larva). It eats and grows for about 25–30 days, moulting its skin four times. Each stage between moults is an instar; it stops eating and lifts its head, motionless, for about a day at each moult. By the end it is 7–8 cm long and has grown about 10,000 times heavier than when it hatched. About four-fifths of all its eating happens in the last stage.
- Cocoon. The full-grown caterpillar stops eating, turns slightly translucent, and searches for a corner. It then spins for 2–3 days, swaying its head in figure-eights, pushing out a liquid from two glands that hardens in air into a double strand of protein (fibroin) coated in a gum (sericin). One cocoon is a single filament roughly 600–1,500 m long.
- Pupa inside the cocoon, for about 10–14 days.
- Moth. The moth softens one end of the cocoon with a fluid and pushes out through it — spoiling the filament so that it can never again be unwound in one piece. The moths mate, the female lays 300–500 eggs, and both die within days, without eating.
To reel a cocoon as one thread you must therefore kill the pupa before the moth emerges — by heat, usually. Cocoons that are allowed to hatch are used for breeding, and their broken silk is spun like wool.
The gum (sericin) glues the filament to itself in the cocoon. Hot water softens it so that the filament can be unwound. Later, the gum is boiled off with soap (degumming), which leaves the soft, lustrous, white silk.
What you need
| Item | Amount | Notes |
|---|---|---|
| Mulberry trees | 10–20 well-grown trees, or a hedge of 100–200 bushes | White mulberry is best. Pick leaf from established trees only |
| Silkworm eggs | About 1 g (1,500–2,000 eggs) for a first season | See Where to find it |
| Mulberry leaves | About 20–30 kg per 1,000 caterpillars | Fresh, clean, dry |
| Rearing trays | Shallow trays of woven reed or bamboo, about 1 × 0.6 m, on a rack | 1,000 full-grown worms need about 1.5–2 m² |
| Mounting frames | Bundles of twigs or straw, or a grid of cells of folded paper or woven straw | Where they spin |
| Room | Clean, shaded, airy, kept at 23–28 °C | Free of ants, rats, birds, smoke and lizards |
| Reeling pot and reel | A pot over a small fire; a wooden reel about 1–1.5 m round | See below |
What you get. A fresh cocoon weighs about 1.5–2 g. Roughly 5,000–6,000 cocoons give 1 kg of reeled silk, which needs about 150–200 kg of leaves. A silk shirt needs perhaps 100–150 g of silk — around a thousand cocoons.
Where to find it
- Mulberry trees. White mulberry (Morus alba) is native to northern China and has been planted for silk across Asia, the Mediterranean and the Americas, often near old farms, towns and railway embankments. Black mulberry (Western Asia) and red mulberry (eastern North America) feed silkworms too, but less well. Leaves are shiny, toothed, heart-shaped, and often wildly different in shape on one tree — some plain, some lobed like a mitten; cut twigs bleed white sap; the fruit looks like a long blackberry. Grow new trees from cuttings 20–30 cm long pushed into moist soil in late winter, or from seed. Keep them pruned low so leaves are easy to pick.
- Silkworm eggs survive only where people keep them: China, India, Japan, Korea, South-east Asia, Central Asia, Turkey, Brazil, and in small numbers in Italy, France, Spain and the Balkans, and among schoolchildren and hobbyists everywhere. Eggs can be stored in a cool place (about 5 °C — a cellar or cave in winter) for months.
- Wild silks, if no domestic eggs can be found:
- Tussah (Antheraea species) feed on oak, and spin large brown cocoons in China and India; reelable with effort.
- Eri silkworms (Samia ricini) feed on castor-oil plant leaves in north-east India; their cocoons are open at one end and are spun, not reeled.
- Muga of Assam give a golden silk; African wild silk moths (Anaphe, Gonometa) make communal nests or cocoons of usable silk.
- Search trees in late summer and autumn for cocoons: tough, papery, silky, often hanging from a twig or wrapped in leaves. Many wild cocoons are stiffened with minerals and must be softened by boiling in weak lye or ash water before use.
Step by step
1. Grow the mulberries first
Plant trees or a hedge three to five years before your first big rearing. Feed them with manure (Compost and Manure), and prune hard each winter to make lots of young shoots. Never strip a young tree bare.
2. Hatch the eggs
- In spring, when the mulberry buds burst, bring the eggs into the warm rearing room (about 25 °C) and keep the air moist. They turn dark blue-grey a day or two before hatching. Hatching takes about 10–14 days.
- The newly hatched worms are black, hairy and about 3 mm long ("ants"). Lay a sheet of thin cloth or paper with small holes over the eggs and scatter finely chopped tender leaves on top: the worms climb up through the holes onto the leaf. Lift the sheet onto a tray.
3. Rear the caterpillars
- Feed 3–5 times a day, morning to late evening. Chop leaves finely for the first two instars, coarsely for the third, and give whole leaves or leafy shoots after that.
- Leaves must be fresh, clean and dry. Pick them in the cool morning after the dew has dried, keep them in a cool, damp (not wet) cellar or under a damp cloth, and never feed wet, dusty, yellowed or fermented leaves. Wet leaves cause disease.
- Give them room. Spread the worms out at every moult so they never pile up. Their space needs to roughly double at each moult.
- Clean the beds every day or two in the later stages. Lay a net or a sheet of perforated paper over the worms with fresh leaf on top; they climb up, and you lift them off the old droppings and stalks.
- Leave them alone during moults. When most worms are still with raised heads, stop feeding until they have all moulted, then feed again. Dust the bed with dry slaked lime (Lime) or wood ash at moults; it dries the bed and checks disease.
- Keep the room at 23–28 °C, warmer and moister for the young worms, cooler (23–24 °C) and drier for the last stage. No direct sun, draughts, smoke or strong smells.
4. Mount them to spin
At the end of the fifth instar — after about 6–8 days of very heavy eating — the worms stop eating, turn slightly yellow and see-through, and wander about raising their heads. Pick them up and set them on mounting frames: bundles of dry twigs, straw rolled into spirals, or grids of cells about 3 × 4 cm. Stand the frames upright so droppings fall clear. Keep the room airy and not too humid. In 2–3 days the cocoons are finished.
Harvest the cocoons about 7–8 days after the start of spinning: the pupa inside is then formed and firm. Strip the loose outer floss and sort the cocoons. Set aside the best — firm, heavy, evenly shaped, from healthy batches — for breeding (step 7).
5. Stifle the pupae
Before the moths emerge (about 10 days after spinning began), kill the pupae:
- Steam the cocoons in a basket over boiling water for about 15–20 minutes, then dry them in the shade; or
- Dry-heat them in a warm oven or kiln at about 60–80 °C for several hours, until a cocoon rattles when shaken; or
- Sun them on hot days, spread on cloth, for 3–4 days.
Dried cocoons keep for months if stored dry, away from rats and insects. This step kills an animal; if you cannot accept that, see Peace silk below.
6. Reel the silk
- Cook a handful of cocoons in water just under the boil (about 90–95 °C) for 2–5 minutes, pushing them under, until they soften and sink. This loosens the gum.
- Find the ends. Brush the floating cocoons gently with a small whisk of rice straw or twigs. Loose strands catch on the whisk; pull them up and peel away the tangled outer layer until each cocoon gives a single clean filament that runs freely.
- Lower the heat so the reeling water stays hot but not boiling, about 40–60 °C.
- Gather 5–10 filaments together into one thread. One filament alone is far too fine to use. The more cocoons, the thicker the thread.
- Pass the thread through a guide — a small eyelet of glass, smooth bone or metal, fixed above the pot — and then cross it round itself (or round a second thread) for several twists before it goes up to the reel. This crossing squeezes out water and presses the filaments together so they stick into one round thread.
- Wind it on a reel turned by a crank — a wooden frame like a large spool, 1–1.5 m round, turned at a steady pace. A guide that moves slowly from side to side (driven by a cam or an eccentric peg on a gear from the crank, see Cranks, Cams and Linkages) lays the thread in a broad crisscross so wet turns do not lie on each other and stick.
- Feed in new cocoons as each one runs out or breaks: throw the end of a new filament onto the running thread and it sticks by its own gum. Keep the number of filaments constant so the thread stays even.
- Dry the skeins on the reel before taking them off.
A practised reeler with a helper turning the reel can reel a few hundred grams of raw silk a day.
7. Breed next year's eggs
- Let the moths emerge from the cocoons you set aside (10–14 days after spinning). The males flutter their wings constantly.
- Pair each female with a male for 3–4 hours, then separate them.
- Set each female on a piece of paper or cloth, under an upturned cup, to lay her eggs.
- Disease check: the deadly disease pébrine passes from mother to egg. Crush each mother after laying and look at her body fluid under a The Microscope (×400): if you see many small, shiny, oval spores, burn her eggs. Without a microscope, keep each female's eggs separate, note which families rear healthily, and breed only from healthy lines.
- Keep the eggs cool and dry until spring.
Degumming and spun silk
Raw reeled silk is stiff and dull because of the gum. Boil it gently in water with plenty of soap — about 1 part soap to 4 parts silk by weight, in water to cover — for about an hour, then rinse well. It loses about a quarter of its weight and becomes soft and shining. Soapwort works too (Wool). Do not use strong lye: like wool, silk is a protein and lye destroys it.
Spun silk uses everything that cannot be reeled: cocoons the moths have broken (sometimes called peace silk, since the moth lives), double cocoons, outer floss and reeling waste. Degum it, then card or comb it and spin it like wool (Spinning and Weaving Cloth). Cocoons can also be boiled and stretched over a small frame into thin layers ("silk hankies") that pull out easily into a spinnable strand.
How to tell it worked
- Healthy worms are pale, plump, eat vigorously, and the bed sounds like gentle rain when they feed. Sick worms are sluggish, shrunken, spotted, soft, or chalky.
- Good cocoons are firm, heavy for their size, evenly shaped, and rattle faintly (the pupa) when shaken.
- Good raw silk is an even, smooth, round thread. When you break a single strand it resists surprisingly hard. It burns slowly, smelling of burnt hair, leaving a crushable black bead.
Note Troubleshooting. Worms die soft, black and smelly (flacherie) → wet, fermented or dirty leaves, heat, crowding. Clean more often, feed only fresh dry leaves, give more space. Worms die stiff and covered in white or green mould (muscardine) → damp. Lower humidity, dust with lime, burn dead worms. Worms with black pepper-like spots, uneven growth → pébrine. Burn the whole batch and start again from tested eggs. Filament breaks constantly while reeling → under-cooked or over-cooked cocoons, or cocoons from sick worms. Cook more evenly; reel cooler. Skeins stuck in hard lumps → the guide was not traversing, or the thread was too wet. Cross the thread more, reel more slowly.
Dangers
- Heat and steam. Reeling pots and steaming baskets scald. Keep children away; lift cocoons with a ladle or whisk.
- Allergies. Some people develop asthma or skin rashes from silkworm dust, moth scales or the steam of the reeling pot. Keep rooms airy; those affected should do other work.
- Pesticides and smoke. Silkworms are killed by tiny amounts of smoke, insecticides, and tobacco: never use any near the trees or the rearing room.
- Fire. Drying cocoons in an oven or kiln can scorch and ignite them. Keep the heat low and steady.
What this unlocks
Silk thread for Sewing, Needles and Thread, sutures for Basic Surgery, and fishing lines for Fishing. Silk-covered wire for Copper Wire, The Electromagnet and The Telegraph instruments. Fine bolting cloth for flour and powder sieves (Grain, Flour and Bread). Varnished silk for gas bags and Balloonss, and later for parachutes and the fabric skins of some early Gliders and Aeroplanes. Silk's example — a long, strong protein fibre drawn from a liquid — inspired the first artificial fibres (Rayon and Nylon).
How it was first done
Chinese tradition credits Leizu, wife of the Yellow Emperor, with discovering silk when a cocoon fell into her tea. Archaeology agrees silk began in China: chemical traces of silk proteins have been found in tombs at Jiahu in Henan about 8,500 years old, and woven silk fragments from Qianshanyang in Zhejiang date to about 4,700 years ago. For thousands of years China guarded the secret, trading silk west along the routes later called the Silk Road. Around AD 552, according to the Byzantine historian Procopius, monks smuggled silkworm eggs from Central Asia to Constantinople, probably hidden in hollow canes, starting European silk-making. In the 1860s a disease (pébrine) almost destroyed the French and Italian silk industries until Louis Pasteur showed that it spread through the eggs and devised the microscope test for mothers described above — one of the first victories of germ science.
Source: content/entries/textiles/silk.md