Part 13 · Electricity
Thermocouples and Thermoelectricity
Join two different metals and heat one junction, and a small, steady voltage appears that rises with the temperature. That is the thermocouple — the way almost every furnace, kiln and engine has been measured since the 1890s. How to choose the metals, make the wires and junction, calibrate it against melting metals, read furnace heat to a few degrees, build thermopiles that sense radiant heat or give a steady current, and use a flame to hold a gas valve open.
- Difficulty
- ●●●●●
- Time
- An afternoon for a copper–constantan couple; a day to make, calibrate and fit a furnace thermocouple; a week for a thermopile generator
- Steps from zero
- 19 prerequisites →
This unlocks
—The full path from nothing — 19 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- Hides and Leather
- Fermentation
- Bellows
- Copper Smelting
- Iron (the Bloomery)
- Blacksmithing
- The Battery
- Copper Wire
- The Electromagnet
- Measuring Electricity
- Thermocouples and Thermoelectricity
Do them roughly in this order. See it on the tech tree →
Why it matters
A glass The Thermometer breaks at a few hundred degrees. Above that, potters, smiths, glassmakers and steelmakers judged heat by the colour of the glow, by clay cones (Pyrometric Cones and Kiln Temperature) and by pieces of metal that melt — good methods, but rough, slow and hard to write down (The Thermometer, The Kiln). A thermocouple — two wires of different metals joined at the tip — reads the heat inside a furnace directly, continuously and from a distance, to within a few degrees, at anything from freezing to 1,500 °C.
That lets you:
- Fire Pottery, Glazes, Stoneware and Porcelain and Bricks the same way every time.
- Harden and temper Steel and Alloy and Stainless Steels at the right heat, and anneal Glass without cracking it.
- Watch the temperature of Boilers and Pressure Vessels, engine exhausts (The Internal Combustion Engine) and chemical reactions (Distillation).
- Build a flame-failure valve that shuts off gas if a burner goes out (Biogas and Wood Gas).
- Detect faint radiant heat — from a person, a star, an invisible beam (Detecting Radiation).
- Make a small, steady current from a flame, with no moving parts and no chemicals.
It needs only two kinds of wire and a sensitive meter (Measuring Electricity), so it is one of the most useful things you can make once you have copper wire.
How it works
The Seebeck effect
Make a loop of two different metals — say copper and iron — joined at both ends. Heat one joint and keep the other cool. A current flows round the loop for as long as one joint is hotter than the other. Break the loop and put a sensitive meter in the gap: it reads a small voltage, which grows with the difference in temperature between the hot joint (the hot junction, or measuring junction) and the cool one (the cold junction, or reference junction).
The voltage is tiny: a few hundredths of a thousandth of a volt per degree — measured in microvolts per degree (µV/°C), or in millivolts (mV) in all. But it is steady and repeatable: the same two wires at the same temperatures always give the same voltage.
Which metals?
Each metal has a place in the thermoelectric series. The farther apart two metals are in this list, the more voltage they give together:
| Metal (near room temperature) | µV/°C, compared with platinum |
|---|---|
| Antimony | +47 |
| Iron | +19 |
| Copper, silver, gold | +6 to +7 |
| Platinum | 0 |
| Nickel | −15 |
| Constantan (55% copper, 45% nickel) | −35 |
| Bismuth | −72 |
Subtract to get a pair's voltage: iron against constantan gives about 19 − (−35) = 54 µV/°C; copper against constantan about 42 µV/°C; bismuth against antimony nearly 120 µV/°C.
The best pairs give a large, steady voltage that rises evenly with temperature, and survive the heat:
| Pair | About | Good up to | Notes |
|---|---|---|---|
| Copper – constantan | 40–43 µV/°C | 350 °C | Ovens, boilers, dryers, low heat. Copper oxidises above this |
| Iron – constantan | 52–55 µV/°C | 750 °C | The best first furnace couple. Iron rusts away above this |
| Nickel-chromium – nickel-aluminium | about 41 µV/°C | 1,200 °C | Needs chromium and aluminium alloys (Alloy and Stainless Steels, Aluminium) |
| Platinum – platinum with 10% rhodium | 6–12 µV/°C | 1,500 °C | Glass and steel furnaces; very costly but very stable |
| Copper – iron | 12 µV/°C, falling | 250 °C only | Easy, but its voltage stops rising at about 270 °C and then falls: never use it for furnaces |
| Bismuth – antimony | about 110 µV/°C | 150–200 °C | Very sensitive; for thermopiles that detect radiant heat |
Two rules that make it practical
- Only the ends matter. The voltage depends only on the temperatures of the two junctions, not on how hot the wires are along the way. So the wires can pass through a furnace wall and out across a hot room.
- A third metal adds nothing if both its ends are at the same temperature. So you can solder or braze the junction, and join copper leads to run to the meter, as long as the two joins where the copper meets the thermocouple wires are at the same temperature — side by side in the cold-junction bath.
The reverse: the Peltier effect
Drive a current through a junction of two metals and it warms or cools slightly, depending on the direction. With metal pairs the effect is weak; with certain semiconductor crystals it is strong enough to freeze water and is used for small coolers (Semiconductors and the Transistor, Ice and Refrigeration).
What you need
| Item | Notes |
|---|---|
| Iron wire, 1.5–3 mm for furnaces, 0.5 mm for quick readings | Soft, clean iron (Iron and Brass Wire) |
| Constantan wire, same size | 55 parts copper to 45 nickel by weight (below) |
| Copper wire | For leads and copper–constantan couples (Copper Wire) |
| Insulators | Two-hole clay tubes or strings of fired clay beads (Pottery, Firebrick and Refractories) |
| Protective sheath | Iron pipe closed at one end (to 800–900 °C), or a fired porcelain or fireclay tube (higher) (Stoneware and Porcelain) |
| Millivoltmeter | A moving-coil meter reading 0–50 mV, with high resistance (below) (Measuring Electricity) |
| Cold-junction flask | An insulated jar of crushed ice and water |
| Pure metals for calibration | Tin, lead, zinc, aluminium, a little silver |
| Small crucibles and charcoal powder | For melting the calibration metals (Metal Casting) |
Where to find it
- Nickel for constantan comes from garnierite — a soft, bright apple-green ore in weathered red-brown soils over dark green serpentine rock (New Caledonia, the Urals, Oregon) — or from sulfide ores of the same rock family; smelting and refining it is in Nickel and Cobalt.
- Copper: native copper and green and blue ores (Copper Smelting). Iron: bog iron, magnetite and other ores (Iron (the Bloomery)).
- Antimony from stibnite — lead-grey, needle-like crystals that melt in a candle flame; bismuth from silvery, pinkish native bismuth and from bismuthinite (Antimony and Bismuth).
- Platinum — heavy, silvery-grey grains in some river gravels with gold (Platinum and the Platinum Metals); rhodium for the platinum–rhodium couple is separated from the same crude metal (Palladium, Rhodium and Iridium).
- Zinc from calamine and sphalerite (Zinc and Brass).
Step by step: an iron–constantan furnace thermocouple
1. Make the constantan
- Melt 55 parts copper in a covered crucible under a layer of charcoal powder, in a furnace that reaches about 1,300 °C (white-yellow heat) (Metal Casting).
- Add 45 parts nickel in small pieces. Nickel melts at 1,455 °C, but it dissolves in hot molten copper. Stir with a fireclay rod; skim.
- Cast into a rod mould. Draw it into wire through steel draw plates, annealing it at a red heat every few passes (Iron and Brass Wire).
- Keep a note of each batch. Every batch is a little different, so calibrate each one (step 4).
Without nickel, a copper – iron couple will do for ovens and drying below 250 °C, and that is all.
2. Make the junction
- Cut a length of iron wire and of constantan wire, each long enough to reach from the hottest point in the furnace to outside it, plus 20–30 cm.
- Clean 3 cm at one end of each, bright with emery.
- Twist the two ends together tightly for 2–3 turns.
- Fuse the tip. Connect the twisted pair to one terminal of a 12–24 V battery or a welding transformer (Welding); connect a pointed carbon rod (from an arc lamp or a battery) to the other. Touch the rod to the very tip and draw it away: the arc melts the tip into a small, round, shiny bead. Cut off any loose ends below the bead. For use below about 700 °C you can instead braze or silver-solder the twist (Soldering and Brazing).
3. Insulate, sheath and connect
- Thread both wires through two-hole clay tubes or strings of small fired clay beads, so the wires cannot touch each other anywhere except at the bead. Make tubes by extruding fine clay through a die with two pins, drying and firing them (Pottery).
- Slide the whole into a protective sheath closed at the hot end, with the bead touching the end. Bare iron and constantan wires corrode quickly in furnace gases; the sheath gives them a long life.
- At the cold end, join each thermocouple wire to a copper lead with a twisted, soldered joint. Put both joints together in a small glass tube standing in a jar of crushed ice and water — exactly 0 °C. This is the cold junction.
- Run the copper leads to the millivoltmeter.
Without ice: let the cold junction sit at room temperature, measure the room with an ordinary The Thermometer, and add the room temperature to your reading. It is accurate to a few degrees for iron–constantan.
4. Calibrate it
A home-made couple will not exactly match any table. Calibrate it against things whose temperatures are fixed by nature.
- Ice point: hot junction in crushed ice and water → 0 mV. (If not, check for a stray junction somewhere.)
- Boiling water: about 100 °C at sea level, about 1 °C less for every 300 m of altitude.
- Freezing points of pure metals. Melt 200–500 g of a pure metal in a small crucible, under a layer of charcoal powder to keep air off. Push the sheathed thermocouple deep into the melt. Turn off the heat and read every 15–30 seconds as it cools. The reading falls, then stops falling and holds steady for several minutes while the metal freezes — the heat given out by freezing holds the temperature still. That steady reading is the metal's freezing point.
| Metal | Freezes at |
|---|---|
| Tin | 232 °C |
| Lead | 327 °C |
| Zinc | 420 °C |
| Antimony | 631 °C |
| Aluminium | 660 °C |
| Common salt (melted) | 801 °C |
| Silver | 962 °C |
| Gold | 1,064 °C |
- Plot the millivolts against the temperatures on squared paper and draw a smooth curve through the points. Read any later millivolt value off the curve, or make a table and paint it on a board beside the furnace.
For comparison, a standard iron–constantan couple with its cold junction at 0 °C reads about: 5.3 mV at 100 °C, 10.8 at 200, 16.3 at 300, 21.8 at 400, 27.4 at 500, 33.1 at 600, 39.1 at 700. Yours should be within a few percent.
5. The meter
The voltage is small, so the meter matters.
- Use a moving-coil meter reading 0–50 mV full scale for iron–constantan to 750 °C (Measuring Electricity).
- Give the meter a resistance at least 100 times that of the thermocouple and its leads (a couple and leads might be 1–3 Ω; so the meter should be 200–300 Ω or more). Then the reading hardly changes when the wires heat up or you lengthen the leads.
- Calibrate the couple and meter together, with the same leads, and never change one without recalibrating.
- For the best accuracy, measure with a potentiometer — balance the thermocouple's voltage against a known, adjustable voltage until the galvanometer reads zero (Measuring Electricity). No current flows, so wire resistance does not matter at all.
Thermopiles
Join many couples in series, with all the odd junctions on the hot side and all the even ones on the cold side, and their voltages add: a thermopile.
As a heat detector. Twenty to fifty tiny bars of bismuth and antimony (or fine bismuth and antimony wires), their hot ends blackened with soot and set behind a polished metal cone, feeding a sensitive galvanometer. It detects the warmth of a hand at a metre and measures the heat in sunlight or in the invisible infrared beyond the red of a spectrum (The Spectroscope). Keep it shielded from draughts. Bismuth melts at 271 °C: never put it in a flame.
As a current source. A flame or a stove can drive a thermopile to give a steady, quiet current for a The Telegraph, a small Electroplating bath, or charging a battery, with no chemicals to replace.
- Elements: cast bars of a zinc–antimony alloy (about 35 parts zinc to 65 antimony by weight; melt the antimony under charcoal, then add the zinc), each about 10 cm long and 1 cm square. Join each bar's ends to strips of iron (or constantan) by casting the bar onto the strip.
- Arrange them in a ring round a gas or charcoal burner, hot junctions inward, cold junctions outward with thin copper or iron fins to shed heat (or dipped in a water jacket).
- Keep the hot side below about 400 °C — the alloy melts at about 550 °C, and runs better if not pushed.
- Expect roughly 0.05 V per pair with 300 °C between the hot and cold sides, so 40–60 pairs give 2–3 V.
Be honest about the cost: a metal thermopile turns less than 1% of the fuel's heat into electricity. It is worth it only where a steady, maintenance-free current matters more than fuel. Semiconductor materials do several times better (Semiconductors and the Transistor).
The flame-failure valve
A simple, life-saving use: a valve on a gas line (Biogas and Wood Gas) that is held open only while the flame is lit.
- Put a short, thick iron–constantan thermocouple, sheathed in a thin iron tube closed at the tip, in the edge of the pilot flame. It slowly burns away; replace it when the valve starts to drop out on its own.
- Connect it directly to a small electromagnet wound with a few turns of thick copper — its resistance must be tiny, a hundredth of an ohm or so, because the couple gives only 20–30 mV (The Electromagnet).
- The magnet is too weak to pull the valve open, but strong enough to hold a soft-iron plate on a spring-loaded valve once it is pushed against it. To light the burner, press a button that pushes the plate against the magnet and lets gas through; light the pilot; hold for 30–60 seconds while the couple heats; release.
- If the flame blows out, the couple cools within a minute, the magnet lets go, and the spring snaps the valve shut.
How to tell it worked
- Zero at the ice point: both junctions in ice water reads 0 mV.
- Steady and repeatable: the same furnace, the same heat, the same reading day after day; the freezing plateaus of tin, lead and zinc fall on a smooth curve.
- Agrees with nature: a scrap of zinc, aluminium or salt on a tile beside the bead should melt just as the reading passes its melting point (The Thermometer lists these sentinels).
- Responds quickly: lifting a sheathed couple out of a furnace makes the reading fall within seconds to a minute.
Note Troubleshooting. Reading goes backwards (needle below zero) → wires reversed at the meter; swap the leads. Reading drifts lower over weeks → the hot end is oxidising or the alloy is changing; cut off the end, re-bead, and recalibrate. Use a sheath. Reading jumps when you touch or move the leads → a loose joint, or one of the copper–thermocouple joints is warmer than the other; put both together in the cold bath. Reading too low compared with cones or colours → the bead is not at the hottest point, the sheath is too thick, or the meter's resistance is too low. Push it in farther; use a high-resistance meter. Reading stops rising above about 270 °C → you are using copper–iron; change to iron–constantan. No plateau when calibrating → the metal is impure (it freezes over a range), or too little metal; use a purer metal and at least 200 g.
Dangers
Danger Molten metal and furnaces. Calibrating means handling crucibles of molten tin, lead, zinc and aluminium. A damp tool or a wet crucible makes molten metal explode out. Dry and preheat everything; wear leather and a face shield. Lead and antimony fumes are poisonous and zinc fumes cause metal fume fever: melt outdoors, upwind, and do not overheat (Lead, Antimony and Bismuth, Zinc and Brass). Never melt metals in kitchen pots.
- The fusing arc is bright enough to burn the eyes: look through dark glass (Welding).
- A wrong reading can be dangerous: an over-fired kiln or a boiler thought to be cooler than it is. Check thermocouples against cones and sentinels from time to time (The Thermometer).
- Gas valves must be tested: blow out the flame on purpose and check the valve closes within a minute before trusting it.
Going further
- Base-metal couples for higher heat: nickel–chromium against nickel–aluminium reaches 1,200 °C in air.
- Platinum couples for glass and steel furnaces; a single gram of platinum makes a fine wire couple that lasts years (Platinum and the Platinum Metals, Palladium, Rhodium and Iridium).
- Recording: a meter needle that presses on a turning paper chart every minute writes a whole firing's temperature history (Instruments, Chart Recorders and Control Rooms).
- Automatic control: a contact on the meter needle can switch a relay to open or close a damper or fuel valve, holding a kiln at a set heat (Thermostats and Automatic Control, Process Controllers and Control Valves).
- Radio and electrical meters: a tiny heater with a thermocouple on it measures alternating and radio-frequency current by the heat it makes (Radio).
- Semiconductor thermoelectric generators give several times the efficiency, enough to run radios from a kerosene lamp (Semiconductors and the Transistor).
How it was first done
In 1821 the Estonian-German physicist Thomas Johann Seebeck, working in Berlin, found that a compass needle swung near a closed loop of bismuth and copper when he warmed one of the joints. He believed he had found a way that heat made magnetism; Hans Christian Ørsted soon showed that a current was flowing and named it thermoelectricity. The Italian Leopoldo Nobili built a thermopile around 1829, and Macedonio Melloni used it in the 1830s to show that radiant heat behaves like light. The French watchmaker and physicist Jean Peltier discovered the reverse heating and cooling effect in 1834, and in 1838 Emil Lenz froze a drop of water on a bismuth–antimony junction with it. William Thomson (later Lord Kelvin) worked out the theory linking the effects in the 1850s.
In 1886 Henri Le Chatelier in Paris introduced the platinum / platinum-rhodium thermocouple, and within a few years it was the standard way of measuring the heat of furnaces, kilns and steel. Gas-fired thermopiles by Charles Clamond (1870s) and Gülcher (1890) powered electroplating and telegraphs. In the 1950s the Soviet physicist Abram Ioffe led work on semiconductor thermoelectric materials that powered radios from kerosene lamps; similar generators heated by radioactive decay still power deep-space probes such as Voyager, launched in 1977.
Source: content/entries/electricity/thermoelectricity.md