◆ Rebuild

Part 8 · Chemistry

Composites: Fibreglass, Carbon Fibre and Honeycomb

Strong fibres set in a hardening resin make a material that is light, rot-proof, and can be moulded to any shape. How fibre and resin share the load, how to make a mould and lay up fibreglass panels and boat hulls by hand, how carbon fibre is made from rayon or acrylic fibre, and how a honeycomb core between two thin skins gives a panel hundreds of times stiffer for about a third more weight.

Difficulty
●●●●●
Time
An afternoon for a first flat panel; two to four weeks of evenings for a dinghy plug, mould and hull; carbon fibre needs a factory
Steps from zero
15 prerequisites →

You need first

Glass Fibre and Glass WoolEarly Plastics

This unlocks

Resins: Phenolic, Polyester and Epoxy
The full path from nothing — 15 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. The Kiln
  5. Pottery
  6. Lime
  7. Lye and Potash
  8. Fermentation
  9. Glass
  10. Saltpeter
  11. Distillation
  12. Glass Fibre and Glass Wool
  13. Sulfuric Acid
  14. Nitric Acid
  15. Early Plastics
  16. Composites: Fibreglass, Carbon Fibre and Honeycomb

Do them roughly in this order. See it on the tech tree →

Why it matters

Glass fibre is stronger than steel for its weight, but a loose bundle of it is floppy. Resin on its own is stiff but brittle and cracks like toffee. Together they make fibreglass: light, strong, waterproof, rot-proof, and able to take any shape a mould can give it. One person with a bucket and a brush can make a boat hull, a water tank, a roof light, a car body or a wind-turbine blade with no forge, no rolling mill and no welding.

Composites are any material built of strong fibres in a binding matrix. People have used them for millennia: mud bricks reinforced with straw, plaster with hair, the horn-wood-sinew bow (Bow and Arrow), plywood, Reinforced Concrete. This chapter covers the modern ones: fibre and plastic resin.

What they lead to: boats that never rot or rust (Boats and Sails), car and lorry bodies (The Motor Vehicle), tanks and pipes for acids and water, safety helmets, fishing rods and vaulting poles, limbs for Crutches, Prosthetics and Rehabilitation, blades for wind turbines, parts for Gliders and Aeroplanes, and, with carbon fibre, the lightest strong structures ever built (Spaceflight and Spacecraft).

How it works

Fibre carries the pull; resin holds the fibres. A glass or carbon fibre is immensely strong along its length. The resin glues the fibres together, passes load from one fibre to the next, stops them buckling when squeezed, and keeps out water. Neither does the job alone.

Fibres work only along their length. Laid all one way, fibres give huge strength in that direction and almost none across it. Cloth woven at right angles gives strength both ways. Random mat gives moderate strength every way. Lay fibres along the lines of the load.

More fibre, less resin, is stronger, up to the point where there is not enough resin to wet every fibre. Air bubbles and dry fibres are weak spots.

Material Density (g/cm³) Tensile strength (MPa) Stiffness (GPa)
Polyester resin alone 1.2 50–70 3–4
Chopped strand mat laminate, 30 % glass 1.4–1.5 80–100 6–8
Woven roving laminate, 50 % glass 1.7 200–250 15–20
Carbon fibre in epoxy, all one way 1.55 1,500–2,000 130–150
Mild steel 7.85 about 400 210
Aluminium alloy 2.7 250–300 70
Spruce, along the grain 0.45 70–100 10

The lesson in the last column: fibreglass is strong but floppy, ten to thirty times less stiff than steel. A fibreglass panel must get its stiffness from shape: curves, ribs, and above all sandwich construction, where two thin skins are held apart by a light core. A beam's stiffness rises with the cube of its thickness. Two 1 mm skins held 20 mm apart are about 300 times stiffer than the same 2 mm of laminate in one sheet, for the weight of the core.

What you need

Item Notes See
Glass reinforcement Chopped strand mat (fibres 5 cm long, random, held with a soluble binder) 300–600 g/m²; woven roving (coarse cloth of untwisted bundles) 400–800 g/m²; fine glass cloth for surface layers Glass Fibre and Glass Wool
Resin Polyester, epoxy or phenolic: below Early Plastics, Petrochemicals and Modern Plastics
Catalyst and accelerator for polyester From a chemical works
Release agent Hard wax; polyvinyl alcohol (PVA) solution; or cellophane sheet Rayon and Nylon
Gelcoat Thickened, pigmented polyester for the outer surface
Tools Brushes, laminating rollers, buckets, scales to 1 g, a measure for catalyst, scissors, knife
Mould materials Timber, plywood, plaster, filler, sandpaper Basic Woodworking, Gypsum and Plaster of Paris
Cores Balsa, cork, paper or aluminium honeycomb Below
Safety Goggles, rubber gloves, charcoal-filter respirator, dust masks, eye-wash water

The resins

Polyester resin is the workhorse. A thick, honey-coloured syrup that is two-thirds polyester and one-third styrene, a solvent that also joins in the hardening. Add 1–2 % (by weight) of a liquid peroxide catalyst, and it sets in 15–30 minutes at 20 °C and is hard in a day. A cobalt accelerator (a fraction of a percent) is usually pre-mixed by the maker. It shrinks 5–8 % as it cures, smells strongly, and costs least. Making it needs phthalic anhydride (from naphthalene, Coal Tar Chemicals), maleic anhydride and a glycol, cooked together at about 200 °C until thick, then thinned with styrene. That is a job for a resin works (Organic Synthesis and Fine Chemicals, Petrochemicals and Modern Plastics).

Epoxy resin comes as two parts, a resin and a hardener, mixed in an exact ratio by weight or volume (often 2:1 to 5:1; follow the maker). It is stronger, sticks far better, barely shrinks, and does not smell, but costs several times as much. Wrong ratios never cure properly. It is the resin for carbon fibre, repairs, and wood–epoxy boats.

Phenolic resin (the Bakelite family) is the one a young chemical industry can make first, from phenol and formaldehyde (Early Plastics, Methanol and Formaldehyde; the resin kettle and laminating press are in Resins: Phenolic, Polyester and Epoxy). It does not cure at room temperature: cloth is soaked in the liquid resin, dried until tacky, stacked and pressed hot (about 150 °C) for an hour or so. It is fire-resistant and good at high temperatures, but dark, brittle and gives off water as it cures, so it needs pressure to be free of pores. Phenolic glass or cotton boards make electrical panels, gears and bearings.

Danger Never mix polyester catalyst directly with cobalt accelerator. The two react violently and can explode. Add accelerator to resin, stir well, then add catalyst to that, or buy resin with accelerator already in. Store catalyst in its own vented bottle away from heat and metals. A splash of catalyst in the eye can blind: wash for 15 minutes at once.

Fibreglass mould

Everything starts with a mould: the shape the part takes. For a few parts, the mould can be any smooth, waxed surface. For a run of identical parts (boats, tanks, car panels), make a proper mould from a plug.

  1. The plug is an exact model of the finished object. Build it from timber frames and battens, plywood, plaster or clay (Basic Woodworking, Gypsum and Plaster of Paris). Fill and sand it to a perfect shape: every dent and ripple will show on every part. Seal it with several coats of varnish or shellac and polish it to a gloss (Pigments, Paints and Varnish).
  2. Draft: sides must taper slightly outward, at least 2–3°, or the part will jam. No undercuts. A shape that cannot be pulled straight off is made as a split mould in two or more pieces bolted together along flanges.
  3. Wax the plug: 5–8 coats of hard wax, each buffed, then a coat of PVA if you have it.
  4. Tooling gelcoat 0.5–0.8 mm thick, then laminate the mould about twice as thick as the parts it will make: 6–8 mm for a dinghy mould.
  5. Stiffen it with ribs of timber or steel tube bonded on the outside, and a cradle to stand it level. A mould that flexes makes distorted parts.
  6. Cure for a week, then part it from the plug with wooden wedges and water.
  7. Prepare the mould: cut and sand flanges, polish the inside, and wax it 6–8 times before the first part. Wax lightly before every part after.

A good mould has a mirror finish, keeps its shape when you stand on its cradle, and releases parts with gentle wedging.

Laminating roller

A laminating roller squeezes resin into the mat and drives out the air. It is a row of steel washers or ridged discs on a spindle, with a handle. The ridges press the air out sideways instead of trapping it.

  • Make one: on a 6 mm steel rod, thread alternately 25 mm washers and 15 mm spacers, 10–15 of each, held by nuts. Bend a wire or rod handle and fit a wooden grip. Or turn a solid aluminium or steel cylinder with grooves 2 mm apart (The Lathe).
  • Make one 75 mm wide for flat areas and one 20 mm wide for corners.
  • Clean it in acetone (Ether, Acetone and Solvents) before the resin gels, every time.

A good roller turns freely, has no sharp burrs to tear the mat, and leaves the laminate an even, see-through green with no white streaks.

Fibreglass panel

A flat panel is the first project, and good practice for everything else.

Next layer of mat resin stippled in, then rolled Wetted glass mat each 450 g/m² layer ≈ 1 mm Rolled down hard no white fibres, no bubbles Gelcoat 0.4–0.6 mm, left until tacky Wax or PVA release 5–8 coats on a new mould Mould waxed glass, metal or plywood Hand lay-up, layers pulled apart lay each layer while the last is still tacky; no more than 3–4 at once The finished part is lifted off the mould; the gelcoat becomes its glossy outer face.
Fig. 1 Hand lay-up, layer by layer. On a waxed mould goes the gelcoat, then glass mat wetted with resin, rolled down hard to drive out air, then more layers. The finished laminate is lifted off with the gelcoat as its glossy face.
  1. Work at 18–25 °C, dry, out of direct sun. Below 15 °C polyester cures badly; above 30 °C it gels too fast.
  2. Mould: a sheet of glass, polished metal or smooth plywood, waxed 5 times and buffed, or covered with tight cellophane. Mark the panel's outline with tape.
  3. Cut the mat 2–3 cm oversize, one piece per layer. Tear, don't cut, the edges where pieces overlap, so the joins are feathered. Overlap joins by 5 cm and stagger them between layers.
  4. Gelcoat (optional, for a smooth face): brush on an even coat 0.4–0.6 mm thick (about 500 g/m²). Wait until it is tacky but does not come off on a finger: 30–60 minutes.
  5. Mix resin for the first layer only: about 2–2.5 times the weight of the mat. For a 1 m² panel of 450 g/m² mat, about 1 kg of resin. Add 1.5 % catalyst (15 g, about 13 mL), stir for a full minute, scraping the sides.
  6. Wet out: brush a coat of resin on the mould, lay on the mat, and stipple (dab, don't stroke) more resin through it from above. The binder dissolves and the mat goes from white to translucent.
  7. Roll firmly from the middle outwards until no white fibres or silver bubbles remain.
  8. Next layers: repeat while the last is still wet or just tacky. Do no more than 3–4 layers of 450 g mat at once. A thicker wet stack overheats as it cures, can crack, smoke, and even catch fire.
  9. Trim the edge with a sharp knife when the laminate is "leathery", about 30–60 minutes after gelling, before it goes hard.
  10. Cure 24 hours, then lift it off with plastic wedges. It reaches full strength in a week at room temperature, or in a few hours at 60 °C.

Thickness: each layer of 450 g/m² mat makes about 1 mm of laminate. A panel for a roof light or tank side: 3–4 mm. For a load-bearing floor, use a sandwich (below).

Woven roving is laid alternating with mat (roving, then mat, then roving) because roving alone does not bond well to itself. A mixed laminate has about 40–45 % glass and is roughly twice as strong as mat alone.

Fibreglass boat hull

Fibreglass boats need no caulking, swell no seams, and never rot. Hand lay-up in an open mould is still how most small boats are built.

Mould flange wedges go in here Fibreglass mould 6–8 mm, twice the hull Timber cradle keeps the mould true Gunwale strip hardwood, bonded in Topsides 3 layers, about 3 mm Bottom 4–5 layers, 4–5 mm Gelcoat outer face, 0.5 mm Stringers wood or foam, every 30–40 cm, covered with two layers of mat Keel 3 extra strips
Fig. 2 A fibreglass dinghy hull in section, in its female mould. The mould is a stiff fibreglass shell on a timber cradle. Inside, the hull laminate is thickest along the keel and transom. Stringers of wood or foam, covered with fibreglass, stiffen the bottom; a gunwale strip stiffens the edge.

For a 3.5–4.5 m rowing or sailing dinghy:

  1. Plug and mould as above. A female mould (the hull is built inside it) gives a gloss outside. The mould needs a gelcoat of the hull's colour.
  2. Gelcoat the mould, 0.5 mm.
  3. Skin coat: one layer of light mat (300 g/m²) rolled extra carefully. Air just under the gelcoat makes blisters later.
  4. Laminate schedule (each "layer" = 450 g/m² mat, or equivalent mat and roving):
    • Topsides: 3 layers, about 3 mm.
    • Bottom: 4–5 layers, about 4–5 mm.
    • Keel line, stem, transom and chines: 3 extra strips, 10–20 cm wide, laid first. Wherever there is a corner or a fitting, add.
  5. Stiffeners: while the laminate is still tacky, set stringers along the bottom: strips of timber or foam 25–40 mm deep, every 30–40 cm, covered with two layers of mat lapping 5 cm onto the hull. Add frames or bulkheads of plywood bonded in with mat tape, and a gunwale strip of hardwood or a folded laminate flange around the top edge.
  6. Buoyancy: sealed compartments under the seats, or blocks of cork or foam, so the boat floats when swamped (Life Jackets, Lifebuoys and Lifeboats).
  7. Cure a week before release. Pull it out with wedges and water, or air blown between hull and mould through a valve built into the mould.
  8. Trim the edges with a fine saw, sand and fit the gunwale, seats, rowlocks and fittings bolted through with large washers or wooden pads (Boats and Sails).

A dinghy of this kind weighs 50–80 kg. A one-off boat without a mould can be built over a male frame of battens covered in a skin of cloth or foam, laminated outside, then turned over and laminated inside. It needs much more sanding and filling to get a fair surface.

A good hull: even thickness (drill small test holes in trim offcuts and measure); no soft spots when you press the bottom; a sharp, ringing sound when tapped with a coin all over, not a dull thud; gelcoat free of blisters and star-cracks.

Honeycomb core and honeycomb panel

The sandwich. A light core between two thin, stiff skins, glued together, gives a panel that is very stiff and very light. The core must resist shearing and crushing, and the glue must hold the skins to it.

Core Density (kg/m³) Notes
End-grain balsa 100–250 Small blocks glued edge to edge with the grain upright. Excellent, and strong in crushing. Rots if water gets in
Cork 120–250 Damp-proof, damps sound; flexible
Paper honeycomb dipped in resin 30–80 Cheap and very light; doors, partitions, aircraft floors
Aluminium honeycomb 30–100 The aircraft standard
Foam (PVC, polyurethane) 40–200 Modern boats and wind blades (Petrochemicals and Modern Plastics)
1 Glue stripes, staggered2 Press, then slice the block3 Pull each slice open4 Glue skins on both faces glue stripe s widestripes every 4 sstripes on every second sheet shifted 2 sPaper or foilsheets, edge-on Slicesas thick as thecore: 10–25 mmfront face: sheets edge-on,as in 1 Orange: glued double walls. Free walls openinto hexagons; s = 5–6 mm gives 10 mm cells. Skin1–2 mm laminateCore10–25 mmSkinTwo 1 mm skins 20 mm apart: about 300 times stifferthan the same 2 mm of laminate in one sheet.
Fig. 3 Making a honeycomb core by the expansion method. Strips of glue are printed across sheets of paper or foil, staggered half a step on alternate sheets. The stack is pressed and the glue set, the block is sliced across the glue lines, and each slice is pulled open into hexagonal cells. Two skins glued to the faces make the panel.

Making honeycomb core by the expansion method:

  1. Cell size. Choose the side length of a cell wall, s: 5–6 mm gives cells about 10 mm across.
  2. Glue lines. On a sheet of strong kraft paper (Paper, Wood Pulp, Kraft Paper and Paperboard) or thin aluminium foil (Aluminium), apply stripes of glue s wide, spaced 4 s apart, running the full length of the sheet. Use a printing roller or a comb-spreader. On every second sheet, shift the stripes 2 s sideways.
  3. Stack 50–200 sheets, alternating the two patterns, press between boards, and let the glue set.
  4. Slice the block across the glue lines into strips as thick as your core: 10–25 mm. Use a bandsaw or a sharp knife guided by a fence.
  5. Expand: pull each strip open sideways. The unglued spans open into hexagonal cells. Pin the expanded sheet on a board.
  6. Paper core: dip it in thin phenolic or polyester resin, drain, and cure to make it rigid and damp-proof.

Making a panel:

  1. Lay up one skin on a waxed flat mould: for a floor, 2 layers of 450 g/m² mat.
  2. While it is still tacky, press the core into it, weighted evenly with boards and bags of sand.
  3. When cured, glue or laminate the second skin onto the other face.
  4. Close the edges with a strip of wood or a laminate return, so water cannot reach the core.

A panel of two 2 mm glass skins on a 20 mm paper honeycomb weighs about 7 kg/m² and is stiff enough to walk on over a span of a metre.

Good and bad: tap it all over; a hollow, rattling patch means the skin has come away from the core (delamination). Press the skin with a thumb; it should not dimple. Cut through an offcut: every cell wall should end in a fillet of resin on both skins.

Carbon fibre

Carbon fibre is a thread of almost pure carbon, 5–10 thousandths of a millimetre thick: three to five times stiffer than glass fibre and lighter. In epoxy it makes racing bicycles, aircraft wings, rocket cases and satellite structures stiffer than steel at a fifth of the weight. It is also an excellent electrical conductor and heat-resistant.

The simple version. Carbonise a thread of cotton, rayon or bamboo by heating it, packed in powdered charcoal in a sealed iron or clay box, slowly up to bright red heat, 1,000 °C, and cooling it shut (Charcoal, The Kiln). Edison's lamp filaments were made this way (The Light Bulb). The fibre conducts and survives high heat, so it serves for heating elements, electrodes and filters. But it is weak: the molecules are jumbled, and the fibre shrinks and cracks unevenly.

Strong carbon fibre, in outline. The secret is to hold the fibre under tension at every stage, so its carbon sheets line up along it.

  1. Starting fibre: rayon (Rayon and Nylon) gave the first strong carbon fibres. Today, nearly all use PAN (polyacrylonitrile, the acrylic fibre of knitting wool, from a petrochemical works).
  2. Stabilise: pass the fibre through air ovens at 200–300 °C for 1–2 hours, held taut. It turns black and stops melting.
  3. Carbonise: pull it through a furnace filled with nitrogen (Liquid Air, Nitrogen and the Noble Gases) at 1,000–1,500 °C for a few minutes. Everything but the carbon is driven off as gas. About half the weight of PAN survives; only a quarter of rayon.
  4. Graphitise (for the stiffest grades): a second furnace at 2,000–3,000 °C.
  5. Surface treat by passing it through a weak electrolytic bath so resins stick to it, then size it with a thin coat of epoxy, and wind it on spools as tows of 1,000–50,000 filaments.

Each step needs precise temperature control over long furnace lines (Electric Kilns and Furnaces). A carbon-fibre plant is a major industrial undertaking.

Using carbon fibre: always with epoxy; laid along the load path, often as unidirectional tape or as woven cloth. Parts are laid up by hand like fibreglass, or as resin-soaked "prepreg" sheets cured under vacuum in a heated pressure vessel (an autoclave, Pressure Vessels and Valves).

Good and bad: a good tow is glossy black, its filaments parallel and unbroken; a fuzzy, dull tow with broken ends is weak. A good laminate shows a uniform weave with no dry patches or ripples.

How to tell it worked

  • Look through a laminate held up to light before gelcoat: an even translucent colour. White patches are dry glass; silver specks are air.
  • Tap test all over with a coin: crisp ringing is sound; dull thudding is delamination or a void.
  • Hardness: a fingernail should not mark cured polyester. A surface still tacky after two days means too little catalyst, too cold, or air-inhibited (polyester stays tacky where it touches air unless the last coat contains wax).
  • Burn-off test: weigh a 5 cm offcut, burn it in a crucible at red heat until only white glass remains, and weigh again. The remaining glass should be 25–35 % of the weight for mat, 40–55 % for mixed laminate. Much less: too much resin, weak and brittle.
  • Bend an offcut until it breaks. It should crack with fibres pulled out like a brush, not snap clean like glass.

Note Troubleshooting. Won't cure, stays sticky → too little catalyst, too cold below 15 °C, or old resin. Gels in the pot → too much catalyst, too hot, or too big a batch; mix smaller batches. White spots and soft patches → dry glass; stipple more resin and roll harder. Blisters in gelcoat → air under the skin coat, or water soaking in through a thin gelcoat. Part sticks in the mould → not enough wax, a new mould not run in, or no draft. Cracks and smoke in a thick lay-up → too many layers at once; build up in stages. Print-through, the weave showing on the gelcoat → gelcoat too thin, or laminated before it was tacky.

Dangers

Danger Styrene vapour causes headache, dizziness and drunkenness, and in a closed space can make a worker collapse. It is also highly flammable; its vapour is heavier than air. Laminate with plenty of through-draught, wear a respirator with an organic (charcoal) filter for large jobs, and keep every flame and spark away. Cured resin dust and cutting smoke are also harmful.

Danger Heat and fire. A bucket of catalysed resin left to set can overheat, smoke and burst into flame. Never leave mixed resin in a bucket; spread leftovers thinly on a scrap of metal to cure. Store catalyst cool and separate.

  • Glass dust and fibre itch and irritate skin and lungs. Wear long sleeves, gloves, and a dust mask when cutting or sanding. Wash in cold water first so pores close.
  • Epoxy causes allergy that builds with each exposure until even its smell brings a rash. Never let it touch skin.
  • Carbon fibre dust conducts electricity and shorts out motors and switchgear. Cut it with vacuum extraction, away from electrical equipment.
  • Moulds are heavy and awkward. Lift hulls with enough people or a hoist (Lifts, Hoists and Mine Winding).

Going further

Filament winding (resin-wet fibre wound on a turning mandrel) makes pipes, pressure tanks and rocket cases. Vacuum bagging, sealing a wet lay-up under plastic sheet and pumping out the air (The Vacuum Pump), gives more fibre, less resin and no fumes. Flax or hemp cloth in resin makes cheaper panels where strength matters less. The same methods build Wind Turbines blades, Gliders and Aeroplanes parts, Crutches, Prosthetics and Rehabilitation and sports gear (Games and Sports Equipment).

How it was first done

Games Slayter at Owens-Illinois in the United States made continuous glass fibre in the early 1930s; Owens-Corning sold it as "Fiberglas" from 1938. Carleton Ellis patented unsaturated polyester resins in 1936, and Pierre Castan in Switzerland and Sylvan Greenlee in the United States developed epoxies in the late 1930s and 1940s. In 1942 Ray Greene of Toledo, Ohio, built one of the first fibreglass-and-polyester boats, and wartime radar domes, which needed a material radio waves could pass through, spread the method. The 1953 Chevrolet Corvette had the first mass-produced fibreglass car body. Hugo Junkers patented a honeycomb core in 1915, and the de Havilland Mosquito (first flown 1940) had plywood skins on a balsa core. Thomas Edison carbonised cotton and bamboo for lamp filaments in 1879–80. Roger Bacon at Union Carbide made strong graphite filaments in 1958; Akio Shindo in Japan made carbon fibre from PAN in 1961; and in 1963 William Watt, Leslie Phillips and William Johnson at the Royal Aircraft Establishment, Farnborough, found that stretching the fibre while heating it made it far stronger and stiffer.

Source: content/entries/chemistry/composites.md