◆ Rebuild

Part 2 · Earth and Fire

Slip Casting, Jiggering and Ceramic Factories

Pour liquid clay into a plaster mould and the plaster drinks the water, leaving a thin, even clay skin in exactly the mould's shape; spin clay on a plaster mould under a steel profile and a plate forms in seconds. How to make casting slip with a deflocculant, make and use plaster moulds, build the jigger and jolley, and set up the pug mill, filter press and production line of a pottery factory.

Difficulty
●●●●●
Time
A week to make a model and first moulds; a day to mix and rest slip; each casting takes about an hour, but dozens run at once
Steps from zero
19 prerequisites →

You need first

The Potter's WheelGypsum and Plaster of Paris

This unlocks

—
The full path from nothing — 19 steps before this one
  1. Fire
  2. Stone Tools
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Pottery
  9. Charcoal
  10. The Kiln
  11. Hides and Leather
  12. Gypsum and Plaster of Paris
  13. The Wheel and Axle
  14. Bellows
  15. The Lathe
  16. Copper Smelting
  17. Bronze
  18. Bearings and Lubrication
  19. The Potter's Wheel
  20. Slip Casting, Jiggering and Ceramic Factories

Do them roughly in this order. See it on the tech tree →

Why it matters

A thrower on the The Potter's Wheel makes perhaps fifty mugs a day, after years of practice. Plaster changes that. Pour liquid clay into a dry plaster mould and the mould does the shaping: a teapot with its spout, an oval dish, a figure, a toilet bowl or a thin chemist's crucible, each the same as the last, made by someone who learned the job in a week. Spin a lump of clay on a plaster mould under a steel blade and a dinner plate forms in ten seconds. Add machines that prepare clay by the tonne, and the village potter becomes a factory.

The same methods make electrical insulators (Insulators, Cables and Electrical Fittings), laboratory porcelain (Burners, Stands and Laboratory Equipment), sinks and toilets (Toilets, Sinks, Baths and Showers), and the advanced ceramics of Zircon and Zirconium and Piezoelectric Crystals and Ceramics.

How it works

Plaster is a sponge. Set plaster of Paris (Gypsum and Plaster of Paris) is a mass of tiny interlocking needles; about half its volume is fine pores. Dry plaster pulls water out of anything wet that touches it, as a cloth draws up water.

Slip casting. Pour runny clay (slip) into a dry hollow mould. Water is sucked into the plaster and the clay particles pile up against the wall as a firm skin. The skin thickens fast at first, then slower: a wall twice as thick takes four times as long, because the water must pass through the skin already formed. When it is thick enough, pour the rest of the slip out. As the skin loses more water it shrinks away from the plaster and lifts out.

Why slip needs a deflocculant. Clay is made of tiny flat plates. In plain water they cling together loosely like a house of cards (they flocculate), so clay flows only when it holds 60–70 parts of water to 100 of clay. Such a slip soaks the mould, casts slowly, shrinks a lot and cracks. A pinch of a sodium compound, a deflocculant, gives all the plates the same electric charge so they push apart and slide past one another. Then a slip with only 35–45 parts of water to 100 of clay pours like cream: faster casting, drier moulds, less shrinkage, fewer cracks.

Use water glass (sodium silicate, Water Glass (Sodium Silicate)) and soda ash (sodium carbonate, Soda Ash and Baking Soda) together. Too little and the slip is thick; too much and it thickens again and casts a soft, flabby wall. Calcium undoes the effect: hard water, lime and crumbs of plaster all spoil a slip.

Jigger and jolley. A lump of soft clay is pressed onto a spinning plaster mould by a fixed steel profile tool. The mould shapes one face, the profile the other, and the plaster then drinks enough water for the piece to shrink free.

What you need

Item Amount Notes
Plaster of Paris 10–20 kg to start Fresh and dry (Gypsum and Plaster of Paris)
Clay body, dry 10 kg per batch of slip Recipes below
Water glass syrup and soda ash 30–40 g and 10–20 g per 10 kg of dry body Use rain water if yours is hard
A model of the piece One Turned plaster, carved wood, or trimmed clay
A fine sieve (lawn) 0.2 mm mesh or finer Brass wire or silk cloth (Iron and Brass Wire, Silk)
A 1-litre measure and a balance Balances, Steelyards and Weighing Machines
A spinning head for the jigger 250–400 turns a minute Belt from a The Watermill or The Electric Motor

Bodies that cast well, by dry weight. Kaolin casts fast; very sticky clay casts slowly and sticks.

Body Plastic clay Kaolin Ground quartz or flint Ground feldspar Fires at
White earthenware 25 25 35 15 1,100–1,150 °C
Stoneware 30 25 20 25 1,240–1,280 °C
Porcelain 5–10 45 25 25 1,280–1,320 °C

A local red clay that throws well usually casts well once sieved and deflocculated. See Finding and Preparing Clay and Stoneware and Porcelain for the raw materials.

Casting slip

Casting slip is clay, water and deflocculant, mixed to a fixed weight and flow so it casts the same way every day.

  1. Dissolve 30 g of water glass syrup and 15 g of soda ash in 3.5 litres of warm rain water.
  2. Add 10 kg of dry powdered body slowly, stirring hard. It looks far too thick at first; keep stirring and it loosens. A blunger (below) saves your arms.
  3. Adjust. Still stiff when all the clay is in? Add water glass solution a few drops at a time, stirring a minute between. Too thin? Add dry clay, never water.
  4. Sieve through the lawn, then stir a strong magnet (Magnets) through it to catch iron specks, which burn to black spots.
  5. Rest it a day, covered, so air rises out. Stir gently before use; do not whip in air.

Testing it.

  • Weight of a litre. Earthenware and stoneware slip: 1.75–1.80 kg. Porcelain: 1.70–1.75 kg. Lighter means too much water.
  • Flow. Time 200 ml running out of a tin cup through a 6 mm hole in its base. Note the time when a batch casts well and match every later batch to it. Let a full cup stand one minute and time it again: good slip runs a little slower after standing (it gels slightly at rest — it is thixotropic) but still runs freely. If it sets solid, add deflocculant; if it runs no slower at all, you have probably added too much.
  • By hand. Good slip runs off a lifted stick in a smooth ribbon like thick cream, then breaks into drops. A finger drawn through it leaves a groove that closes in about a second.

Plaster moulds

pour in slip slip hollow surplus to bucket cup 1. Fill Fill the dry mould to the top of the spare in one steady pour. 2. Wait Water soaks into the plaster (blue); a clay skin builds on the wall. 3. Drain Tip it up when the wall is thick enough; let it drip 10–20 minutes. 4. Release The shell shrinks free. Trim the spare, open the mould, lift it out. spare plaster clay skin
Fig. 1 Slip casting in a two-piece plaster mould, in section. 1, the mould is filled to the top of the spare. 2, the plaster drinks water and a clay skin builds on the wall while the slip level drops. 3, the mould is tipped and drained, leaving a hollow shell. 4, as the shell dries it shrinks free and the mould is opened.

A plaster mould for casting is a block of absorbent plaster with a cavity the shape of the outside of the piece, split into as many parts as the shape needs to come out, and topped by a funnel-shaped reservoir, the spare. Basic one- and two-part moulds are in Gypsum and Plaster of Paris; here is what is particular to casting.

The model. Clay shrinks as it dries and fires: earthenware about 8–10 % in length altogether, stoneware 10–13 %, porcelain 13–16 %. So make the model bigger: a porcelain cup to finish 8 cm across is modelled 9.4 cm across (8 ÷ 0.85). Measure your body's shrinkage on a fired test bar with marks 10 cm apart. Plaster makes the best model: pour a solid block, fix it on a wheelhead or The Lathe, and turn it with steel scrapers an hour or two after it sets, while it is still soft.

Mixing plaster. Sprinkle plaster onto water, never the reverse; let it soak 2 minutes, stir gently 2–3 minutes, pour as it begins to thicken. Keep the ratio the same every time, or moulds will absorb differently.

Mould Plaster : water by weight Why
Casting moulds 100 : 70–80 Porous; drinks fast
Jigger and jolley moulds 100 : 65–70 Firmer; takes the profile's pressure
Case moulds (masters) 100 : 40–50 Hard, built to last

Sizes. Walls at least 3 cm thick everywhere, 4–5 cm for anything bigger than a teacup; a thin mould drinks too little and casts weak walls. A spare 3–5 cm tall above the rim. Round keys on every joint face, and parting lines placed on sharp edges of the design where seams are easy to clean.

Block, case and working moulds. A mould gives 50–100 casts before its face softens. To make many identical moulds: make a block mould around the model; pour hard plaster into it to make a case mould, the mould in reverse; then pour as many working moulds inside the case as you need. The case mould is the factory's treasure: soap it, store it dry, never cast slip in it.

Drying. A new mould holds its own weight in water. Dry it for several days in a warm, airy room, never above 45 °C, or the plaster starts losing its own water and turns soft and powdery. It is dry when it no longer feels cold against your cheek. A mould takes two or three casts a day before it is too wet; then dry it overnight. Keep soap and grease off a casting mould's face, and clean it with a damp sponge, never a metal scraper.

Step by step: casting a cup

  1. Assemble the dry, clean mould and band it tight with rubber strips, or cord and wedges.
  2. Fill in one steady pour down the middle, to the top of the spare.
  3. Top up as the level drops. Keep it full.
  4. Check the wall after 8–10 minutes by scraping slip off the spare's edge with a knife point. A cup wants 2.5–3.5 mm, a jug or vase 4–6 mm. Earthenware slip in a dry mould typically reaches 3 mm in 10–20 minutes.
  5. Drain. Tip the mould over a bucket, pour out the surplus, and leave it upside down at a slight tilt for 10–20 minutes. Sieve the surplus back into stock.
  6. Trim the spare level with the mould top once the shine has gone from the inside.
  7. Release. After 30–90 minutes the cast shrinks visibly from the wall. Open the mould and lift it out by its base with dry hands.
  8. Fettle when leather-hard: pare off seam lines with a sharp knife and smooth them with a barely damp sponge. Cast handles solid in their own small moulds and fix them on with slip when cup and handle are equally leather-hard.

Solid casting. For a dish with a thick foot or a toilet bowl with inner channels, the mould has a core as well as an outside, and slip fills the whole gap between them; nothing is poured out. Use slip at the heavy end of the range and generous mould walls.

The jigger and the jolley

The jigger: plates and saucers The jolley: cups and bowls Pivot and stop arm stops at one height Profile tool steel, shapes back and foot Clay plate upside down Plaster mould shapes the face Head 250–400 turns a minute pull the arm down belt from line shaft Pivot and stop Profile tool shapes the inside Clay cup Plaster mould hollow; shapes the outside Head pull the arm down
Fig. 2 Left, the jigger making a plate. A plaster mould shaped like the plate's face sits in a cup on the spinning head; the profile tool, pivoted on its arm, comes down to a stop and shapes the back and foot ring. Right, the jolley making a cup. The mould is a hollow cup that forms the outside; the profile forms the inside.

The jigger

A jigger makes flatware: plates, saucers, shallow dishes.

  • The head: a metal or hardwood cup 25–35 cm across on a vertical spindle turning 250–400 times a minute. Each mould drops in and is held by a taper. Drive it by belt from a line shaft or a 0.5–1 kW motor; a heavy kick wheel (The Potter's Wheel) works for trials.
  • The moulds: plaster humps whose tops are the face of the plate, with a tapered stem beneath. You need 60–150 per jigger for a day's work, because each plate sits on its mould until it dries free.
  • The arm: a stout bar 60–80 cm long, pivoted at the back, with a handle in front and an adjustable stop so it always comes down to the same height.
  • The profile tool: a flat steel blade 3–5 mm thick (Blacksmithing), filed to the exact shape of the plate's underside including the foot ring. Hard maple or boxwood serves for the first few hundred plates.

Making a plate.

  1. Make a bat: beat a weighed lump of soft clay (0.8–1 kg for a 25 cm dinner plate) into a round pancake 6–8 mm thick with a flat wooden spreader.
  2. Throw it onto the mould face and press it down from the centre outward with a damp sponge to drive out air.
  3. Pull the arm down with the head turning, in one steady movement, to the stop. The profile slices away surplus clay and shapes the back. Hold a second; lift. A splash of water helps the cut.
  4. Trim the rim with a wooden sliver as it spins.
  5. Lift off mould and plate together onto a rack at 30–40 °C. In 1–3 hours the plate lifts free.

A team of three — maker, mould runner and batter-out — makes 1,000 or more plates a day.

The jolley

A jolley is the same machine for hollowware: cups, bowls, basins. The mould is a hollow plaster cup that forms the outside; the profile hangs down into it and forms the inside. Drop a soft ball of clay into the spinning mould, bring the profile down to spread it up the walls in one stroke, trim the rim, and set the mould aside to dry free.

Good from bad. A good piece is even in thickness (thin porcelain held to a lamp glows evenly), smooth-faced, and lies flat on a sheet of glass. S-shaped cracks in the base come from trapped air or clay too stiff; press harder and use softer clay. Warping comes from uneven drying. Tearing or chattering at the profile means stiff clay or a blunt tool.

Preparing clay in quantity

lawn magnet pump 4–8 atm clear water out cakes hopper Blunger stirs clay and water into thin slip Filter press cloth-wrapped plates clamped by a screw; water squeezes out, clay cakes stay Pug mill slanted knives chop the clay and push it out of the nozzle as a solid column
Fig. 3 The clay preparation line. The blunger stirs clay and water into slip, which passes through a fine lawn and over magnets to the filter press. Pumped in under pressure, it leaves cakes of clay between cloth-covered plates. The pug mill chops and squeezes the cakes into a solid, airless column for the jigger and jolley.

The blunger

A blunger is a round tub of wood, brick or sheet iron, 1–2 m across, with a vertical shaft carrying paddles that turn 20–40 times a minute. It stirs clay, ground flint, feldspar and water into a thin slip (1.3–1.5 kg a litre) that runs out through a bottom tap, through lawns and over magnets.

The filter press

A filter press squeezes the water out of thin slip. It is a row of 20–60 square plates, 50–100 cm across, of cast iron or hardwood, each with a shallow recess on both faces and a hole through the middle, each wrapped in strong cotton or jute filter cloth (Spinning and Weaving Cloth). A big screw clamps them together in a frame (Screws, Nuts and Bolts) so the recesses form chambers.

  1. A ram or diaphragm pump (Pumps) forces slip into every chamber at 4–8 atmospheres.
  2. Clear water squeezes through the cloths and runs out of a tap on each plate. Milky water means a torn cloth.
  3. After 1–3 hours the water slows to a drip. Release the screw, part the plates, and peel out cakes 2–3 cm thick, holding about a fifth of their weight in water: just right for working.

A small press of ten 40 cm wooden frames makes 100–200 kg of clay a pressing. Before filter presses, slip was dried for days in long heated brick troughs.

The pug mill

A pug mill mixes clay to an even softness and squeezes out air. It is a strong barrel 15–30 cm across and 60–120 cm long, with a shaft along its middle carrying knives set at a slant like a screw thread. Each turn chops the clay and pushes it on toward a tapered nozzle, from which it comes out as a firm, solid column, ready to cut into balls and bats.

  • The simplest is an upright barrel turned by a horse or ox walking a circle (Animal Power and Treadwheels); potteries used them for two centuries.
  • The workshop mill is horizontal, turning 15–30 times a minute through reduction Gears from a 1–4 kW motor or line shaft.
  • A de-airing mill shreds the clay through a perforated plate into a sealed chamber pumped to low pressure (The Vacuum Pump), so air bubbles burst out. De-aired clay is denser and stronger and jiggers far better.

The production line

A pottery factory (a potbank) lays its steps out so clay and ware move one way:

  1. Grinding: flint and feldspar calcined and ground wet in mills (The Watermill); clays weathered outdoors for months.
  2. Slip house: blunger, lawns, magnets, filter press, pug mill. Scraps from every later stage come back here.
  3. Making shops: throwers, jiggerers, casters and pressers, by windows, with drying rooms beside them.
  4. Green shop: fettling, sponging, handles.
  5. Biscuit firing. English earthenware is biscuited hard, 1,100–1,150 °C; stoneware and porcelain soft, 850–950 °C, so they still drink glaze.
  6. Dipping in glaze (Glazes), and the glost (glaze) firing.
  7. Decorating with printed transfers and enamels fixed at 700–800 °C, then sorting: every piece rung, inspected and graded.

Measure every firing with Pyrometric Cones and Kiln Temperature so every load comes out the same. Large works replace batch kilns with tunnel kilns, in which loaded cars creep through a long hot tunnel.

How to tell it worked

  • Castings: walls even when a test piece is sawn in half; no pinholes inside; no cracks at the base or where spouts join; a clear ring when fired and tapped.
  • Slip: same weight and flow time every batch; does not settle hard overnight.
  • Moulds: release within an hour without sticking; leave no plaster crumbs on the clay.

Note Troubleshooting.

  • Casts too thin and slowly → mould wet, slip too thin or overdeflocculated.
  • Casting sticks → mould wet or new; too much sticky clay in the body.
  • Flabby walls that slump on draining → too much deflocculant; stir in some untreated slip.
  • Slip thick in the bucket overnight → too little deflocculant, or plaster crumbs or hard water.
  • Pinholes inside → air in the slip; stir gently, let it stand, pour steadily.
  • Cracks where thick meets thin → uneven shrinkage; design even walls, dry slowly under cloth.

Dangers

Danger Silica dust kills slowly. Ground quartz and flint, dried slip, scrapings and plaster dust hang in a pottery's air. Breathed for years they scar the lungs (silicosis, "potter's rot"), and there is no cure. Fettle and clean wet, never sweep dry; grind flint wet; wear a damp cloth mask where dust cannot be avoided, and ventilate (Ventilation and Air Conditioning).

Danger Machines that pull you in. Pug mill knives and blunger paddles will take a hand and an arm. Never reach into a running pug mill's feed; push clay in with a wooden plunger. Guard belts and gears and put a stop lever within reach (Belts, Chains and Power Transmission).

  • Filter presses hold slip at several atmospheres. Clamp fully before pumping; fit a gauge and relief valve to the pump (Pressure and Vacuum Gauges).
  • Heavy moulds: a wet toilet mould can weigh 50 kg. Lift with two people.
  • Lead glazes were the other great killer of pottery workers; avoid them (Glazes).

What this unlocks

Cheap, fine porcelain and bone china for everyone; laboratory crucibles, dishes and funnels (Burners, Stands and Laboratory Equipment); exact electrical insulators (Insulators, Cables and Electrical Fittings) and spark-plug bodies (The Internal Combustion Engine); sanitaryware (Toilets, Sinks, Baths and Showers); and cast advanced ceramics (Zircon and Zirconium, Piezoelectric Crystals and Ceramics). The model-and-mould discipline carries over to pressed glass (Bottles, Drinking Glasses and Glassware) and to Precision and Interchangeable Parts everywhere.

How it was first done

Clay pressed into fired-clay moulds is ancient: Mesopotamian plaques and Greek and Roman lamps and red tableware were made that way. Plaster moulds came to Staffordshire, England, in the 1740s; tradition credits Ralph Daniel of Cobridge with bringing the idea from France around 1745, and slip-cast salt-glazed teapots and figures followed. Josiah Wedgwood opened his Etruria works in 1769 and organised it as a line of specialist shops, the pattern for ceramic factories since. Horse-driven pug mills and early jiggers belong to the late 18th century; steam-driven jiggers and jolleys spread in the mid-19th, and the clay filter press arrived in the 1850s. Deflocculated slips made with water glass and soda came into wide use around 1900, with cast sanitaryware for the new water closets. De-airing pug mills followed in the 1930s, and automatic roller-head machines replaced the hand jigger from the 1960s.

Source: content/entries/earth/slip-casting.md