◆ Rebuild

Part 15 · Knowledge and Science

Pencils and Chalk

How to make pencil leads from graphite and clay fired in a sealed pot, case them in wood, and make the other dry writing tools — charcoal sticks, chalk, slates, blackboards and wax crayons. Writing that needs no ink, never spills, and costs almost nothing per word.

Difficulty
●●●●●
Time
An afternoon for charcoal sticks, chalk or crayons; 3–5 days to make, dry and fire a batch of pencil leads; a day to case them
Steps from zero
5 prerequisites →

You need first

Basic WoodworkingThe Kiln

This unlocks

—
The full path from nothing — 5 steps before this one
  1. Stone Tools
  2. Fire
  3. Finding and Preparing Clay
  4. Basic Woodworking
  5. The Kiln
  6. Pencils and Chalk

Do them roughly in this order. See it on the tech tree →

Why it matters

Ink is wonderful, but it needs a pen, a pot, a steady table and dry weather, and every mistake is permanent. A pencil writes in the rain, in a pocket, up a ladder and on the side of a plank. Its line can be rubbed out. One pencil writes about 45,000 words or a line some 50 km long, and costs a few grams of mineral and a sliver of wood.

Dry writing tools do jobs ink cannot:

This chapter gives five tools, from easiest to hardest: charcoal sticks, chalk, slates and blackboards, wax crayons, and the true graphite pencil.

How it works

Every dry writing tool is a stick of a soft, coloured solid that rubs off on a rougher surface. Paper fibres, the fine grain of slate, or the grit of a blackboard paint act like a very fine file: they scrape off tiny flakes, which lodge in the surface.

Graphite is a form of pure carbon whose atoms lie in flat sheets, stacked like a deck of cards. The sheets slide over each other at the lightest touch and stick to paper as a dark grey, shiny line. Graphite is also very stable: it does not fade, rot or rust, so a pencil line lasts as long as the paper. (It smudges, though, and can be rubbed off — use ink for anything that must not change.)

Pure graphite is too soft and brittle to make a thin point. In 1795 the French engineer Nicolas-Jacques Conté found the answer that every pencil still uses: grind graphite with fine clay, shape it into rods, and fire them. Firing turns the clay into a hard ceramic skeleton holding the graphite flakes. The ratio decides the pencil:

  • More clay → harder, paler, finer line that keeps its point (called H for hard).
  • More graphite → softer, blacker, smudgier line that wears quickly (called B for black).
  • About 70 parts graphite to 30 parts clay gives a general-purpose medium (HB).

The leads must be fired without air. Graphite burns slowly at red heat in open air, so the rods are packed in charcoal inside a sealed clay pot. Afterwards they are soaked in hot wax or fat, which fills their pores and makes them glide.

1. Clean, weigh, mix 2. Roll and dry 3. Fire without air graphite + fine clay + water,ground for half an hour Hard (2H)60 : 40 Medium (HB)70 : 30 Soft (2B)80 : 20 graphiteclay More clay = harder, paler line Roll under a flat board:rods 2.5 mm, shrink to 2 mm Dry in grooves in the shade,2–3 days, so they stay straight Lidsealed withwet clay Rodsburied incharcoal dust No airor the graphiteburns away Bright orange, ~1,000 °Chold 1–2 hours; cool fullybefore opening, then soak in hot wax
Fig. 1 Making pencil leads. Wash and grind graphite and clay, mix them in the ratio you want, roll them into rods, then fire them packed in charcoal in a sealed pot so the graphite cannot burn away.

What you need

Item For about 50 pencils Notes
Graphite, clean powder 150 g See below. Lump graphite can be sawn into sticks instead.
Fine white or grey clay 50–100 g after washing Finding and Preparing Clay; kaolin (white china clay) is best — free of iron and sand.
Wax or fat 200 g Beeswax, tallow, or a mix.
Clay pot with lid (crucible) One, holding the rods lying flat Or a short length of clay pipe with both ends plugged (Tiles and Clay Pipes).
Charcoal dust Enough to pack the pot Crushed Charcoal.
Kiln or forge Reaching bright orange, ~1,000 °C The Kiln, or a charcoal forge with Bellows.
Soft, straight-grained wood 25 slats, 18 × 7 × 0.5 cm Juniper, cedar, lime (basswood), poplar, alder or willow.
Glue A cup Hide glue (Glues and Adhesives).
Tools Mortar and pestle, pots for washing, smooth flat board, saw, plane or sharp knife, a scratch-stock or small gouge for grooves.

Where to find it

  • Graphite forms in old, heat-and-pressure-changed rocks: schist, gneiss and marble, especially where these contain black streaks. It also forms where coal seams were baked by molten rock. It is dark grey to black, with a dull metallic shine; it is so soft it marks your fingers and paper grey and feels greasy, like soap. It is light for something that looks like metal. Do not confuse it with molybdenite (bluish, heavier, also greasy) or with soft black manganese ores (which leave a brownish-black, not shiny, mark). See Rocks and Minerals and Mining and Tunnelling. Tiny flakes scattered through rock are common; solid lumps are rare treasures.
  • Clay: see Finding and Preparing Clay. White pipe clay or kaolin, found in pockets in weathered granite country, is ideal.
  • Soft wood for casings: trees that carve easily across the grain without splitting — juniper and other "cedars" (reddish, fragrant wood), lime/basswood (pale, soft, even), poplar, alder, willow. Avoid resinous pine (gums the knife) and hard woods (cannot be sharpened with a knife).
  • Chalk: white downs and sea cliffs (see Lime). Gypsum: see Gypsum and Plaster of Paris. Slate: see Quarrying and Cutting Stone. Soapstone: soft, grey-green, soapy-feeling stone you can scratch with a fingernail.

Method 1: Charcoal sticks

The quickest drawing tool of all — and the one cave painters used.

  1. Cut straight willow twigs (or grapevine, spindle or lime) as thick as a pencil, 5–10 mm. Peel off the bark and cut them to 15 cm.
  2. Pack them tightly in a metal tin, or a clay pot with a lid, so they cannot move. Pierce one hole 2–3 mm wide in the lid.
  3. Set it in the hot embers of a fire. Smoke and flame will jet from the hole. After 1–2 hours, when no more smoke comes out, take the tin out and let it cool completely, unopened — opened hot, the sticks burst into flame. This is the same process as Charcoal.
  4. Good sticks are black right through, light, and snap with a clean ring. Brown middles mean underdone; ash means air got in.

Charcoal makes a rich black line that smudges easily. Fix finished drawings by brushing or spraying them with very thin hide glue or gum water.

Method 2: Chalk

  1. Natural chalk. Saw soft, pure white chalk into sticks about 1 × 1 × 8 cm with a knife or old saw. Dry them for a week. Pick chalk without grit or flint — grit scratches the board.
  2. Cast chalk (smoother, less dusty). Mix plaster of Paris with water at about 10 parts plaster to 6–7 parts water by weight, stirring in up to 1 part of powdered chalk for softness, or a pigment (ochre for yellow or red). Pour into moulds: hollow reeds or bamboo split lengthwise and tied back together, or tubes of rolled, greased paper 1–1.5 cm wide, standing in sand. After 30–60 minutes split the mould off. Dry the sticks for 3–5 days.
  3. Soapstone sawn into flat sticks is the metalworker's chalk: its mark survives heat and is visible on dark iron.

Method 3: Slates, slate pencils and blackboards

Writing slates

A slate and a slate pencil were the exercise book of most schoolchildren until about 1900. One slate lasts a lifetime.

  1. Split slate into sheets about 3–5 mm thick (see Quarrying and Cutting Stone). Cut to about 20 × 28 cm by scoring both faces with a hard point and snapping over a straight edge.
  2. Rub both faces flat and smooth on a sandstone slab with water and sand, then finer Abrasives and Grinding Stones, until a fingernail glides over it.
  3. Frame it in four strips of wood, grooved on the inside, pegged at the corners. The frame protects the edges and your hands.
  4. Slate pencils are sticks of softer slate, or soapstone, sawn to 5 × 5 mm and rounded on a stone. They leave a pale grey line. Wipe it off with a damp cloth.

Blackboards

  1. Plane wide boards smooth (see Basic Woodworking) and join them edge to edge with glued and pegged battens behind. A useful size is 1 × 1.5 m.
  2. Make the paint: 1 part soot or lampblack (Ink), 1 part very fine pumice or emery powder (Abrasives and Grinding Stones), bound in warm hide-glue water or in linseed oil (Pigments, Paints and Varnish). The grit is essential: it gives the surface the "tooth" that scrapes chalk off.
  3. Brush on three or four thin coats, letting each dry, and rub the last lightly with a cloth to take off the roughest grains.
  4. A single large slab of slate, smoothed as above, makes the best blackboard of all.

Method 4: Wax crayons and pastels

  1. Melt 2–3 parts beeswax (by weight) in a pot standing in a larger pot of hot water — never over a bare flame. Beeswax melts at about 63 °C.
  2. Stir in 1 part finely ground pigment: soot, ochre, chalk, or any earth colour from Pigments, Paints and Varnish. A little tallow makes softer crayons; a little pine resin, harder ones.
  3. Pour into the same moulds as for cast chalk (greased paper tubes in sand). Cool, peel and wrap each in paper.

Pastels are made without wax: mix pigment with powdered chalk or white clay and just enough thin gum water (gum arabic or plum gum; see Ink) to make a stiff dough; roll into sticks and dry for a week.

Method 5: The graphite pencil

If you find solid graphite

The first pencils, in 16th-century England, were simply sticks sawn from lumps of pure graphite. Saw the lump into square rods about 3 × 3 mm with a fine saw (Files and Saws) and glue each into a square groove in a wooden slat (step 9 below). If the lump crumbles, grind it and use the clay method instead.

Clay-and-graphite leads (the Conté method)

  1. Clean the graphite. Crush the ore to powder in a mortar. Stir it into a big pot of water, wait 30 seconds for the heavy rock grit to sink, then pour the cloudy water into a second pot. Graphite (density about 2.2) settles more slowly than most rock grains (about 2.7). Repeat 3–4 times. Let the second pot stand overnight and pour off the clear water. The black sludge is your graphite. Rub a pinch between your teeth: any grittiness will scratch the paper; wash again.

  2. Clean the clay the same way ("levigation"): stir it into lots of water, wait 1–2 minutes, pour off the milky water, let it settle overnight, and keep only the finest sediment.

  3. Dry and weigh both. Mix them by dry weight:

    Pencil Graphite Clay Use
    Hard (2H) 60 40 Fine drawing, marking wood
    Medium (HB) 70 30 Writing
    Soft (2B) 80 20 Sketching, dark lines
  4. Knead with just enough water to make a stiff dough, like putty. Grind it hard on a stone slab for half an hour — the longer and finer the grinding, the smoother the pencil. Cover it and let it rest a day.

  5. Shape the rods. Roll pieces into rods about 2.5 mm thick under a flat board on a smooth slab, or force the dough through a 2.5 mm hole drilled in metal, bone or hardwood, using a plunger in a tube (a simple extruder, the way pencil leads are still made). Cut to 18 cm.

  6. Dry them straight. Lay them in parallel grooves cut in a board, in the shade, for 2–3 days. They shrink to about 2 mm. Bent rods cannot be cased.

  7. Fire them. Lay the rods in a clay pot on a bed of charcoal dust, cover with more dust, put the lid on and seal the joint with a ring of wet clay. Fire in a The Kiln or forge, rising slowly over 2 hours to bright orange, about 1,000 °C (900–1,100 °C works). Hold it there 1–2 hours. Let the pot cool to cold before opening.

  8. Wax them. Drop the fired leads into melted wax or tallow, kept hot (about 100 °C — the wax moves freely but does not smoke) for 2–4 hours. Lift them out and wipe them.

The wooden casing

1. Cut grooves 2. Lay in leads, glue, press 3. Cut apart and shape 4. Sharpen with a knife Slat 5 mm thick, end viewgrooves 1 mm deep, 8 mm apart Second slat glued on top;saw along the dashed lines Six-sided (will not roll)or round, about 7 mm across Soft, straight-grained wood Lead2 mm, waxed about 18 cm long 7 mm
Fig. 2 Casing pencils. Leads are glued into grooves in one slat, a second slat is glued on top, and the pressed "sandwich" is cut into separate pencils and rounded or made six-sided.
  1. Plane slats of soft wood 18 cm long, 5 mm thick and as wide as you like — 7 cm holds six pencils. Cut parallel grooves half a lead deep (1 mm) along the face, 8 mm apart centre to centre, with a small gouge or a scratch-stock (a notched scraper).
  2. Brush hot hide glue into the grooves, lay in the leads, brush glue over the whole face and press on a second, matching grooved slat.
  3. Clamp between boards with wedges or weights for a day.
  4. Saw or plane between the leads to separate the pencils, then shave each round or six-sided (six-sided pencils do not roll off tables). A finished pencil is about 7 mm across.
  5. Sharpen with a sharp knife, cutting away from yourself, then shape the point on fine sandpaper or a flat stone.

Rubbing out

For centuries pencil was rubbed out with balls of soft bread. Better: a lump of Rubber — that is why it is called "rubber". A block of soft, unfired, dry clay also works.

Other points: silver and lead

Before pencils, artists drew with a metal stylus on a prepared surface. A silverpoint is a short wire of silver set in a wooden holder. It leaves a fine grey line only on a ground of bone ash — bones burned white, ground very fine — in thin hide glue, brushed on paper or a wooden panel. The line slowly darkens to brown as the silver tarnishes, and it can never be erased. Medieval scribes ruled their pages with a plummet of lead or lead-tin; see the danger below.

How to tell it worked

  • Pencil: writes an even grey to black line with no scratching. Press firmly: an HB lead should not snap. Sharpen it: the wood should cut cleanly without splitting, and the lead should stay centred.
  • Line test for hardness: draw a stripe with each batch side by side. Each should be visibly darker than the next harder one.
  • Chalk writes in one stroke without squeaking or scratching and wipes off with a dry cloth.
  • Blackboard: chalk lines are crisp; a damp cloth leaves it black again.
  • Crayons leave colour without crumbling and do not melt in your hand.

Note Troubleshooting. Leads crack or blister in firing → dried too quickly, fired too fast, or air was trapped in the dough. Dry longer; heat more slowly; knead out air. Leads scratch the paper → grit in the graphite or clay. Wash both again and grind longer. Leads pale and hard as stone → too much clay, or fired too hot. Use more graphite. Leads crumble or smear → too little clay, or underfired. Use more clay, fire hotter or longer. Leads came out grey and powdery on the surface → air got in and burned the graphite. Seal the lid better; pack more charcoal. Pencil wood splits when sharpened → wood too hard or the grain runs out at an angle. Use soft, straight-grained wood. Chalk squeaks on the board → hold it at a lower angle or break it shorter; the board may need more grit in the paint.

Dangers

Danger Lead is a poison. Lead points, lead white crayons and red lead (minium) poison slowly: tiredness, stomach pain, a blue line on the gums, damage to the brain and nerves — worst in children. Never give children lead pencils or lead-based pigments, never put pencils in the mouth, and use graphite. See Lead.

Danger Toxic pigments. Do not use vermilion (mercury), orpiment and realgar (arsenic, bright yellow and orange), or emerald green (copper and arsenic) in crayons or chalks that children will handle or that might be chewed. Use earths, soot and chalk.

  • Kiln and forge burns. Sealed pots stay hot for hours. A crucible opened hot lets air reach hot charcoal, which flares up.
  • Hot wax catches fire if overheated and burns skin badly. Always heat it in a water bath; keep a lid nearby to smother any flame.
  • Dust. Grinding graphite, slate and chalk raises fine dust. Grind wet whenever you can, and work outdoors. Long exposure to slate and quartz dust damages the lungs (silicosis).
  • Knives. Cut away from your body and hands when shaving casings and sharpening.

What this unlocks

With pencils, slates and chalk you can teach a whole community to read and write cheaply (Teaching and Schools). Pencils are the tool of Surveying and Levelling, Maps and Mapmaking, Measurement from Scratch, engineering drawing (Technical Drawing) and every design in this book. The same graphite-and-clay mixture, with more clay, makes graphite crucibles that survive molten metal (Firebrick and Refractories, Metal Casting), and graphite rods are used in batteries, arc lamps and the The Electric Arc Furnace. Wax crayons lead naturally to candles, and fixed drawings lead to the printed diagrams of Printing.

How it was first done

People have drawn with charcoal and coloured earth for at least 40,000 years. Romans and medieval scribes ruled lines with lead and lead-tin styluses — which is why we still call a pencil's core its "lead". A large, unusually pure deposit of graphite was found at Borrowdale in the English Lake District, probably in the early-to-mid 1500s; local people first used it to mark sheep. The Swiss naturalist Conrad Gessner described and drew a wooden-cased writing stick in 1565. Borrowdale graphite became so valuable that the mine was guarded and, from 1752, stealing from it was a serious crime. Pencil-making grew into an industry around Nuremberg in Germany in the 1600s and 1700s; the Faber family began there in 1761. When war cut France off from English graphite, Nicolas-Jacques Conté patented his graphite-and-clay leads in 1795; Joseph Hardtmuth in Vienna had worked on a similar idea a few years earlier. Joseph Priestley noted in 1770 that rubber rubs out pencil marks. Writing slates were used for centuries and became universal in schools in the 1800s, along with the classroom blackboard, which spread from Scotland and the United States in the early 1800s. Wax crayons for children became cheap in the early 1900s.

Source: content/entries/knowledge/pencils-and-chalk.md