Part 2 · Earth and Fire
Finding and Preparing Clay
How to find clay in the landscape, test whether it is good enough to use, and clean, mix and knead it into a material you can shape into pots, bricks, kilns and moulds.
- Difficulty
- ●●●●●
- Time
- An afternoon to find and test; one to three weeks to prepare a good batch
- Steps from zero
- 0 prerequisites →
You need first
Nothing — start here.Why it matters
Clay is mud that remembers its shape. Wet, it can be pressed into almost any form. Dried, it holds that form. Fired, it becomes stone that you made yourself — and it never turns back into mud.
That simple fact opens most of this book. Clay becomes Pottery for cooking, boiling Finding and Purifying Water, storing grain and brewing (Fermentation). It becomes Bricks for houses and furnaces, the walls of every The Kiln, the crucibles that hold molten Glass and metal, the moulds for Metal Casting, and the lining of the furnace that turns rock into Iron (the Bloomery). Unfired, it seals a Charcoal mound, plasters a Shelter, and lines a pond so it holds water.
Clay is also the easiest material in this part of the book to find. It is under your feet in most of the world. The work is in recognising good clay, and in preparing it properly so that what you make does not crack.
How it works
Clay is rock that has been broken down by water and weather over thousands of years until its grains are unimaginably small — less than one five-hundredth of a millimetre. (Even fine sand grains are about thirty times bigger, and coarse sand a thousand times.) Most clay comes from feldspar, the pale, blocky mineral in granite and similar rocks.
Clay grains are not round like sand. They are flat, like tiny plates or playing cards. When wet, a thin film of water sits between the plates, and they slide over each other without letting go. This is plasticity — the ability to be bent and shaped without cracking. Sand has none: wet sand holds a shape only until you touch it.
Three things happen to clay as you use it:
- Drying. The water between the plates leaves, and the plates pull closer together. The clay shrinks — usually by 4–8% of its length. If one part dries faster than another, the two parts shrink by different amounts and the piece cracks. Most failures in clay work are drying failures.
- Steaming off. Above 100 °C, the last water trapped in the pores turns to steam. If it is driven out too fast, the steam bursts the piece apart.
- Firing. Between about 450 and 700 °C, water that is chemically locked inside the clay crystals is driven off. The crystals change for good. The piece is now ceramic — a kind of artificial stone. It shrinks a little more. An unfired pot dropped in a puddle turns back into mud; a fired one never will.
Because shrinking causes cracks, potters mix clay with temper — coarse, non-sticky grains (sand, crushed pottery, chopped straw) that hold the clay plates apart. Temper reduces shrinkage, opens paths for water and steam to escape, and stops cracks from running. Getting the right balance of clay and temper is the main skill this chapter teaches.
What you need
| Item | Purpose | Notes |
|---|---|---|
| Digging stick or stone blade | Digging clay out of a bank | A fire-hardened, chisel-ended stick works in damp clay |
| Baskets, hides, or large leaves | Carrying clay | Wet clay is heavy: a bucketful weighs about 20 kg |
| Two or three large containers | Slaking and settling | Fired pots, bark buckets, or pits lined with clay or a hide |
| A sieve | Removing stones and roots | Tightly woven basket, cloth, or grass mat |
| Temper | Opening the clay | Sand, grog (crushed fired pottery), straw, dung, burnt shell |
| A flat, absorbent surface | Drying wet clay | Dry sand covered with cloth, dry bricks, or old pots |
| Water | Everything | Rainwater or clean stream water |
For a first batch of pottery, aim for about 10 kg of prepared clay — about half a bucket. That is enough for six to ten small pots and a few test pieces.
Where to find it
Clay forms where water slows down and lets its finest particles settle, or where rock has rotted in place. Look in these places:
- River and stream banks. Especially the cut banks on the outside of bends, where the water has sliced through old layers, and the quiet, muddy inside of bends. Look for smooth, slick, often grey or blue-grey layers between layers of sand and gravel.
- Lake and pond beds. Ponds that stay full long after rain usually sit on clay — clay does not let water through. In a dry season, the mud at the bottom cracks into a pattern of many-sided plates, each curling up at the edges. Those plates are almost pure clay.
- Under the topsoil. Dig down 30–100 cm almost anywhere in a lowland valley. The dark, crumbly topsoil gives way to a denser, heavier, often yellow, orange or reddish layer. Many subsoils are clay-rich.
- Gullies, landslides and sea cliffs, where erosion exposes fresh layers.
- Rotting granite. In hilly granite country, the rock near the surface may crumble to a pale, gritty mass. Hidden in it are pockets of white kaolin (china clay). It is less sticky than river clay, but it survives very high heat, and it is the base of Stoneware and Porcelain.
- Where the land tells you. Puddles that do not drain; boots that collect heavy, sticky mud; mud that dries to a hard crust on your skin; animal tracks that stay sharp for days.
Colour. Fresh clay can be grey, blue-grey, green-grey, yellow, red, brown, cream or white. Grey and blue clays are usually wet clays that have been sealed away from air. Almost all of them fire to red, orange or brown, because they contain iron. Only clay that is cream or white when dry is likely to fire white.
Tip Dig below the roots. The top layers of any deposit are full of roots, worm channels and sand washed in by rain. Scrape off the surface and take clay from 20 cm or more inside the bank, where it is uniform in colour and feel.
Testing clay in the field
Do these tests on the spot, before carrying anything home. Take a lump the size of a walnut, remove stones, and wet it until it feels like soft butter.
- The feel test. Rub the wet lump between finger and thumb. Clay feels smooth, slippery and sticky, like soap or grease. Silt (finer than sand but coarser than clay) feels silky but not sticky, like flour. Sand feels gritty. Touch a tiny smear to your front teeth: grit you can feel means sand.
- The ribbon test. Squeeze the lump between thumb and the side of your forefinger, pushing it out over your finger into a flat ribbon about 3 mm thick. Let the ribbon hang until it breaks under its own weight.
- Breaks under 2.5 cm — too sandy or silty. Not clay; maybe useful for adobe (see Bricks).
- 2.5–5 cm — lean clay. Usable for bricks and kiln walls; awkward for pots.
- Over 5 cm — fat, plastic clay. Good for pots; will probably need temper.
- The coil test. Roll the clay into a coil as thick as a pencil (about 1 cm) and 15 cm long. Bend it round your finger.
- Wraps without a crack, or with only fine surface lines — good, plastic clay.
- Cracks deeply on the outside — workable with care, or mixed with a fatter clay.
- Breaks into pieces — too short (not plastic enough). Look elsewhere.
- The shrink test. Back at camp, make a flat bar 12 cm long, 3 cm wide and 1 cm thick. While it is wet, press two sharp marks into it exactly 10 cm apart (measure with a marked stick — see Measurement from Scratch). Let it dry for a week in the shade. Measure again, then fire it in a campfire (see Pottery) and measure a third time.
- Total shrinkage of 5–10% (marks now 9–9.5 cm apart): ideal.
- More than about 12%: the clay is very fat; add temper or it will crack.
- The bar warped, cracked or crumbled: add temper, or try another deposit.
- The acid test for lime. Drop vinegar, sour fruit juice or any acid onto dried clay. If it fizzes, the clay contains lime (crushed limestone or shell). Lumps of lime in clay turn into quicklime during firing, then soak up moisture from the air and swell, blowing small craters out of the pot days later. Use only clay that does not fizz, or remove every white grain and fire low.
- The test firing. Nothing beats it. Make three small pinch pots and a few tiles from each promising clay, dry them for a week, and fire them in a hot campfire for two hours. Then soak them in water overnight. Good clay comes out hard, rings when tapped, and does not soften. Write down where each clay came from.
Note Keep a clay diary — the deposit, the date, the tests and the results — on a piece of bark or a fired tile. You will find many clays. The notes are how you will remember which one made the pot that did not crack.
Step by step: preparing clay
Clay straight from the ground usually works for bricks and kiln walls. For pots, clean it. There are two ways: the dry way for clay that is already fairly clean, and the wet way (slaking and settling) for clay full of stones, roots and sand.
The wet way
- Dry it completely. Break the dug clay into lumps the size of an egg and spread them in the sun for one to three days until they are hard and pale. Dry clay breaks down in water far faster than damp clay.
- Slake it. Drop the dry lumps into a container and pour in water until it covers them by a hand's width. Do not stir yet. Within an hour the lumps will hiss quietly, release bubbles, and slump. Leave them overnight. They will collapse into a soft mush on their own. This is slaking.
- Make a slip. Stir the mush with a stick or your hands, adding water until it is like thin cream. This liquid clay is called slip.
- Sieve it. Pour the slip through a tightly woven basket, a cloth stretched over a frame, or a mat of fine grass. Rub it through with your hand. Throw away the stones, roots and leaves left behind.
- Settle out the sand. Stir the sieved slip hard, then wait about one minute. The sand sinks to the bottom first. Gently pour the cloudy liquid on top into a second container, leaving the sandy sludge behind. Repeat twice for a fine clay. (This is called levigation. Save the sand — it is perfect temper.)
- Let the clay settle. Leave the second container still for one to three days. The clay sinks slowly to the bottom, and clear water forms on top. Pour or scoop the clear water off.
- Dry the slip to a workable body. The thick slip is now far too wet to shape. Pour it about 3–5 cm deep onto a cloth laid over a bed of dry sand, onto dry bricks, or into an unglazed fired pot — anything absorbent. Or hang it in a cloth bag in the shade to drip. Turn and fold it once a day. In one to five days it will stop sticking to your hands. Take it off when you can roll a coil that does not sag.
- Store it wet. Wrap it in wet cloth or leaves, or keep it in a covered pot. Clay stored damp for several weeks becomes more plastic, because bacteria and moulds work between the plates. Traditional potters age clay for months.
The dry way
Dry the clay completely, crush it to powder on a flat stone with a wooden mallet or a smooth pebble, and pick out every stone and root. Sieve the powder through a fine basket. Mix it with water in a pit, and tread it with bare feet for 15–30 minutes until it is even. This is quicker, but makes dust (see Dangers).
Adding temper
Most good, sticky clays need temper before they can be made into pots that survive drying and firing. Lean clays may need none.
| Temper | How to make it | Best for | Amount (by volume) |
|---|---|---|---|
| Sand | Sieve river sand; use grains up to 1 mm. Angular sand grips better than round beach sand. Wash beach sand to remove salt. | General pots, bricks | 15–30% |
| Grog | Crush broken fired pottery or bricks on a flat stone; sieve. | The best all-round temper; cooking pots; kilns; crucibles | 15–40% |
| Straw, chaff, dry grass | Chop into pieces 1–5 cm long (shorter for pots). | Adobe bricks, kiln walls, plaster; lightens and binds | 10–30% |
| Dung | Dry cow, horse or donkey dung, crumbled and sieved | Smooth, light pots; insulation; mud plaster | 10–25% |
| Burnt shell | Heat shells in a fire, crush to grit | Cooking pots fired below about 750 °C only | 15–30% |
Rules of thumb:
- Start with 20% temper (one part temper to four parts clay) and do the coil and shrink tests again. Add more if the shrink test still cracks; use less if the coil test now breaks.
- Cooking pots need more and coarser temper (25–35%, grains up to 2 mm). The open texture lets them survive being put on a fire again and again.
- Kiln walls, crucibles and furnace linings need the most (up to half grog or sand, plus straw). They must survive heat, not look pretty.
- Organic temper (straw, dung) burns away in firing, leaving tiny holes. The piece becomes lighter, a better heat insulator, and less likely to crack — but weaker and more porous.
- Shell contains lime. Above about 750 °C it turns to quicklime and causes the same blow-outs as limey clay. Some ancient peoples made excellent shell-tempered pots because their open fires stayed cool.
Wedging
Wedging is kneading clay to make it even all through and to drive out air bubbles. An air bubble in a pot wall expands in the fire and blows a hole. Do it every time, right before you make something.
- Take a lump about the size of a loaf of bread. Sprinkle temper over it if you are adding temper.
- Knead like bread dough: push the far side of the lump down and away from you with the heels of both hands, fold it back towards you, turn it a quarter turn, and push again. Do this 50–100 times.
- Or cut and slam: cut the lump in half with a tight cord or a thin blade, lift one half, and slam it down hard onto the other with the cut faces turned outwards. Repeat 20–30 times.
- Check: cut the lump through the middle. The cut face should be the same colour all through, with no streaks, and no holes or pockets. If you see holes, keep going.
Well-wedged clay feels like firm modelling dough: it bends without cracking, holds a fingerprint, and does not stick to dry hands.
How to tell it worked
- A coil of the prepared clay wraps round your finger without breaking.
- A test pot dries for a week without cracking at the rim or base.
- The shrink bar shrinks no more than about 10% from wet to fired.
- A fired test piece rings when tapped with a stick, and does not soften after a night in water.
Note Troubleshooting. Cracks while drying, especially at the rim or where thick meets thin → too little temper, or dried too fast; add 10% more temper and dry in shade under a cloth. Crumbles when you bend it; coils break → too much temper or sand; mix in some fat clay, or age it longer. Sticks to everything and slumps → too wet; dry it on an absorbent surface for another day. Pots blow apart in the fire → air bubbles (wedge longer) or not dry enough (see Pottery). White specks that pop out days after firing → lime in the clay; see the acid test above.
Dangers
Clay is one of the safest materials in this book, but:
- Collapsing banks. Clay banks undercut by digging can fall without warning, and wet clay is very heavy. Dig from the top down, never tunnel, and never dig alone into a bank taller than your waist.
- Deep mud. Soft clay at the edge of lakes and tidal flats can trap a leg like glue. Test the ground with a pole and spread your weight on a board or branches.
- Dust. Dry clay, grog and sand contain very fine quartz dust. Breathing it for months or years causes silicosis, a lung disease with no cure. Crush and sieve dry materials outdoors, damp them down with water whenever you can, and tie a wet cloth over your nose and mouth.
- Strain. Treading and wedging large amounts is heavy work for back and wrists. Share it.
What this unlocks
With prepared clay you can make Pottery, build a The Kiln, and mould Bricks. Clay seals a Charcoal mound, lines a furnace for Copper Smelting and Iron (the Bloomery), and becomes crucibles for Glass and moulds for Metal Casting. White, heat-resistant clays lead to Firebrick and Refractories. Clay mixed with Lime and fired hot becomes Portland Cement.
How it was first done
People were shaping clay long before they made pots. The oldest known fired-clay objects are figurines from Dolní Věstonice in what is now the Czech Republic, about 26,000 years old — including the famous "Venus" figure. The oldest known pottery vessels come from Xianrendong Cave in southern China, made about 20,000 years ago, probably for cooking. Pottery appeared independently in Japan, Africa and the Americas. Everywhere, potters learned the same lessons this chapter teaches: dig carefully, clean the clay, add temper, and dry slowly.
Source: content/entries/earth/clay.md