◆ Rebuild

Part 6 · Building

Laying Tiles and Mosaics

How to set fired tiles on floors and walls so they stay flat, tight and dry for a century — setting out, the mortar bed, cutting, grouting and waterproof showers — and how to make pictures and hard-wearing floors from small pieces, as mosaic and polished terrazzo.

Difficulty
●●●●●
Time
A small floor in two or three days plus a week of curing; a mosaic panel of one square metre in one to three weeks; a terrazzo floor in two to four weeks
Steps from zero
7 prerequisites →

You need first

Tiles and Clay PipesMortar and Concrete

This unlocks

—
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. The Kiln
  5. Tiles and Clay Pipes
  6. Lime
  7. Mortar and Concrete
  8. Laying Tiles and Mosaics

Do them roughly in this order. See it on the tech tree →

Why it matters

A fired tile is a little slab of stone you make yourself (Tiles and Clay Pipes, Stoneware and Porcelain). Set well, tiles give floors that do not wear, rot or burn, and walls behind stove, sink and bath that shed water and wipe clean. Washable surfaces in kitchens, dairies, hospitals and washrooms cut the spread of disease (Sanitation and Germs, Toilets, Sinks, Baths and Showers). Set badly, tiles crack, lift and let water rot the house unseen. The difference is almost all preparation: a stiff, flat base, a full bed and careful setting out.

Small pieces set in mortar also make mosaic, pictures that last thousands of years. Chips of stone in cement, ground flat and polished, make terrazzo, the hardest-wearing floor you can lay.

How it works

A tile is rigid; it needs a rigid base. If the floor below sags even a millimetre, tiles crack or come loose. Use a concrete slab, stone or brick base, or very stiff timber (Foundations and Floors): under load, joists and boards should sag no more than 1/360 of their span under ceramic tiles (8 mm on 3 m), 1/720 under stone.

The bed must be full. A tile on a few dabs of mortar has hollows that ring "drummy" when tapped and crack under a heavy foot. Every floor tile sits on a solid, full bed.

Grout is not waterproof. The joints are filled with grout, a fine mortar, and water soaks slowly through it. So in a shower the waterproofing goes under the tiles.

Movement. Floors warm, cool, dry and settle. Over a big area the tiles need room to move. Leave a gap of 5–10 mm at every wall and every column, hidden under the skirting. Leave a flexible joint across large floors every 4–6 m indoors and every 2.5–4 m in sunshine or over underfloor heating. Fill these joints with a soft mastic of pitch, or of lime putty and linseed oil, not with hard grout.

What you need

Item Notes
Tiles Flat, square, fired hard (Tiles and Clay Pipes). For floors and showers, fire hot enough that a dry tile soaks up less than about 3–6% of its weight in water (stoneware). Sort them by size, colour and flatness before you start.
Bedding mortar Portland cement and sand, 1 : 3 to 1 : 4 (Portland Cement), or hydraulic lime and sand 1 : 2½ (Mortar and Concrete). Plain air lime is soft and slow; use it only for dry floors.
Grout 1 cement : 1–2 very fine sand for joints wider than 3 mm; cement with a little fine sand for narrow ones. Colour with earth pigments (Pigments, Paints and Varnish).
Tools Straightedge 1.5–2 m; spirit level or water level (Surveying and Levelling); chalk line; large wooden square; laying trowel; notched trowel; wooden beating block and mallet; wooden or rubber float; sponges; buckets; tile cutter and nippers (below); kneeling pad.

Setting out

Setting out (plan) 3 4 5 door Chalk lines between midpoints of opposite walls 3–4–5 check 60, 80 and 100 cm: the lines are square Dry-laid tiles light = cut tile at wall; shift the lines until it is at least half a tile Mortar-bed floor (section) Tileswith grouted joints cement paste (the bond) Mortar bed1 : 4, 3–5 cm slurry on the base Concrete slab 5–10 mm gap at the wall, hidden by the skirting
Fig. 1 Setting out a floor. Find the middle of the room with two crossing lines, check them square with a 3-4-5 triangle, and dry-lay tiles both ways. Shift the lines so the cut tiles at the walls are at least half a tile. Below, the layers of a mortar-bed floor in section.

Good tiling is planned before any mortar is mixed.

  1. Find the middle. Snap a chalk line between the midpoints of two opposite walls, and another between the other pair.
  2. Square it. From the crossing, mark 60 cm along one line and 80 cm along the other; the diagonal must be exactly 100 cm. Move a line until it is.
  3. Dry-lay a row of loose tiles, with joint gaps, along each line to the walls. If the last tile would be cut to less than half a tile, shift the line by half a tile. Slivers look poor and break.
  4. Favour the doorway. Put whole tiles where the eye falls first, and the cuts under furniture.
  5. Set the level from a level line round the walls. Floors that must drain fall 1–2 cm per metre to a drain, never toward a door.
  6. Start at the far wall and finish at the door.

The tiled floor

Method 1: The thick mortar bed

This is the old way, and the best on rough or uneven bases. A mud bed of semi-dry mortar is screeded flat, and the tiles are set straight onto it.

  1. Prepare the base: firm, clean and damp, brushed with a cream-thick cement slurry just ahead of the bed so it bonds.
  2. Set screed rails: two straight battens bedded about 1 m apart, tops at bed height and fall, checked with the level.
  3. Mix the bed: 1 cement to 4 sand, just damp enough that a squeezed handful holds its shape but leaves no water on your hand. This semi-dry mix does not slump.
  4. Lay and screed 3–5 cm of it between the rails, pack it, and strike it flat with a straightedge on the rails, about 1 m² at a time.
  5. Make the bond: trowel a thin coat of neat cement slurry over it. This paste glues the tile.
  6. Soak porous tiles 10–20 minutes and drain them, so they do not suck the paste dry.
  7. Set each tile on the line and bed it with taps of a beating block (a board 30 × 15 cm with a handle) until paste just squeezes up. Check with the straightedge; lift a low tile and add paste.
  8. Keep joints straight with a string every few rows, and wedges or card as spacers. Rake joints out to two-thirds depth and sponge the faces as you go.

Keep off the floor for 24 hours. Grout after 1–2 days.

Method 2: The thin bed

On a base that is already flat to within 3 mm under a 2 m straightedge (a well-floated concrete slab or a floated screed), set the tiles in a thin layer of stiff mortar spread with a notched trowel.

The notched trowel is a steel plate about 28 × 12 cm with a handle on the back and square notches filed along its edges (Sheet Metal and Rolling), which comb mortar into ridges of even height: 6 mm notches for tiles up to 20 cm, 10–12 mm for larger.

Comb a stiff mortar of 1 cement to 1–1½ fine sand (a little lime helps it hold) onto the base at 45°, butter each tile back with a thin skim, and press it down with a slight twist. Lift one now and then: the back should be 85% covered on walls and 95% on floors and in showers.

Grouting

  1. Mix grout to a stiff paste, like peanut butter. Let it stand 5 minutes and stir again.
  2. Push it diagonally across the joints with a rubber or wooden float, pressing until the joints are full.
  3. Scrape off the surplus with the float edge held upright, working diagonally so you do not drag grout out of the joints.
  4. After 15–30 minutes, when the grout is firm, wipe the surface with a sponge that is wrung almost dry, in light circles, shaping the joints just below the tile face. Rinse the sponge often.
  5. When dry, polish off the hazy film with dry sacking.
  6. Cure: keep the floor damp under sacking or paper for 3–7 days. Grout that dries too fast powders and cracks.

The tiled wall

  1. The base. Render masonry with 1 cement : 1 lime : 6 sand, floated true to 3 mm under a 2 m straightedge, and let it set a day. Never tile onto gypsum plaster in wet places (Gypsum and Plaster of Paris).
  2. Fix a level batten one tile height above the floor, tile up from it, and fill the bottom row with cut tiles last.
  3. Mark a plumb line set out as for floors, so the corner cuts match.
  4. Set by the thin-bed method, or butter each tile with 5–6 mm of mortar and press and slide it on. Use spacers; do no more than 1 m of height a session, or the low rows creep.
  5. Edges. Finish outside corners with round-edged tiles or a bead. Fill inside corners and the joint at bath or floor with flexible mastic, not grout.

Cutting tiles

Tile cutter push once, far edge to near Handle Scoring wheel hardened, 6–10 mm Breaker Tile glaze side up Rail rubber strip on a hardwood base; fence at the end Snapping (end view) pads press both sides of the score; the ridge under it makes it snap clean Tile nippers hardened jaws meet edge to edge; nibble curves and notches 2–3 mm per bite dotted: next bite
Fig. 2 Cutting tiles. The tile cutter has a hardened wheel that runs along a rail to score the glaze; then the breaker presses down on both sides of the score and the tile snaps cleanly. Nippers nibble curves and notches a few millimetres at a time.

The tile cutter

A fired tile behaves like glass: scratch a line in the glaze and it breaks along it (Window Glass). The tile cutter does this accurately.

  1. Base. A hardwood board about 60 × 25 cm, with a strip of thin rubber or felt glued along it. Fix a raised ridge (a steel rod or hard strip, 3 mm high) down the middle, under the line of cut. Fix a square fence across one end so that tiles sit square to the cut.
  2. Rail. Two steel rods or one stout bar, fixed above the board on end posts, parallel to the ridge.
  3. Scoring wheel. A hardened steel wheel 6–10 mm across, sharpened to a 120–130° edge like a glass cutter's, turning freely on a pin in a sliding block on the rail. Harden it fully and do not temper it much (Steel). A diamond or hardened point scratched along a straightedge works too, but less evenly.
  4. Breaker. A foot on the sliding block, or a separate lever, with two pads that press on the tile either side of the score.

To cut: mark the tile, set it against the fence with the mark over the ridge, and push the wheel across once, with firm, even pressure, from the far edge to the near edge. Never go over a score twice. Then press the breaker down, and the tile snaps cleanly. Smooth the cut edge on a flat sandstone or with a carborundum rubbing block (Abrasives and Grinding Stones).

Tile nippers

Tile nippers are short, stiff pincers with hardened steel jaws that meet edge to edge, 3–4 cm wide. Forge them like heavy pliers (Blacksmithing, Hammers, Pliers, Wrenches and Screwdrivers) and harden only the jaws. Use them to nibble curves and notches around pipes, taking bites 2–3 mm deep from the edge; bigger bites crack the tile.

Thick tiles and stone. Saw them with a plain iron or steel blade fed with wet sand or carborundum grit, or on a spinning abrasive wheel kept wet (Abrasives and Grinding Stones, Gem Cutting and Lapidary). For holes, use a thin-walled iron tube in a bow drill fed with wet abrasive. The tube grinds out a clean round core.

The waterproof shower

A tiled shower floor (section) Wall tiles on cement render Waterproof layer lead, or bitumen and hessian, turned up the walls and over the kerb Grating flush with the tiles Kerb mortar bed Clamping ring with weep holes at the level of the waterproof layer Structural floor pre-slope: 2 cm per metre to the drain solid arrow: water over the tiles dashed: water that seeps through the grout
Fig. 3 A shower floor in section. The structural floor is sloped toward the drain; a waterproof layer covers it and turns up the walls; a mortar bed and tiles go on top. The drain has two levels: water that seeps through the grout reaches the membrane and drains out through weep holes.

A tiled shower that leaks rots the house from inside. The shower tray, the tiled floor of the shower, works like this: a waterproof layer under everything, sloped to a drain that collects water from both the tile surface and the waterproof layer.

  1. Slope the base. Lay a pre-slope screed falling 2 cm per metre to the drain (Pipes, Plumbing and Aqueducts).
  2. The waterproof layer (tanking). Choose one of these:
    • Sheet lead 1.5–2 mm thick (Lead), dressed into a tray with corners folded, not cut, and turned up the walls 15–20 cm (at least 5 cm above the kerb).
    • Bitumen (Tar, Pitch and Glue): two or three coats of hot asphalt or pitch, with a layer of tarred hessian (Flax, Hemp and Linen) between each, also turned up the walls.
    • Fired-clay or stoneware tray made in one piece (Stoneware and Porcelain): the easiest for a small shower.
  3. The drain. Use a two-level clamping drain. The lower flange is clamped to the waterproof layer, and it has small weep holes at that level. The upper grating sits flush with the tiles. Water that soaks through the grout runs down to the membrane, slides along it to the drain and leaves through the weep holes.
  4. Flood test. Plug the drain, fill the tray with water 2–3 cm deep, mark the level, and leave it 24 hours. If the level drops, find the leak now; you will not get a second chance.
  5. The bed. Lay the mortar bed on top, keeping the same fall. Do not block the weep holes; put a ring of coarse gravel around them.
  6. Walls. Make the walls waterproof up to at least 1.8 m. Use cement render (never gypsum), painted with two coats of bitumen or covered with a lime render made waterproof with crushed brick or volcanic ash (Mortar and Concrete). Set the tiles on this.
  7. Tile and grout with dense, low-absorption tiles and a rich cement grout. Fill the inside corners and the joint where wall meets floor with flexible mastic.

Mosaics

A mosaic is a picture or pattern made of small pieces, called tesserae, set in mortar. The pieces can be cubes of coloured stone, fired clay, or glass, or natural pebbles.

Making tesserae.

  • Stone and marble: split strips 1 cm thick into cubes 0.5–1.5 cm across on a hardie (an upright chisel blade set in a log) with a sharp-edged hammer (Stone Carving); the stone breaks cleanly between the two edges.
  • Glass (smalti): melt coloured glass (Glass, Pigments, Paints and Varnish) into flat cakes about 1 cm thick, then cut them on the hardie. Gold tesserae are a thin gold leaf sandwiched between two layers of clear glass (Gold and Silver).
  • Fired clay: roll a slab 6–8 mm thick, score it into a grid, fire it with a glaze (Glazes), and snap it apart.
  • Pebbles: collect flat, rounded beach or river pebbles 1–3 cm across, and sort them by colour.

The direct method (floors, work in place). On a firm concrete or rammed-rubble base, as the Romans did (Mortar and Concrete), draw the design. Spread a setting bed of lime putty with marble dust, or cement mortar, 1–2 cm thick, only 0.1–0.25 m² at a time, and press the tesserae in with 1–2 mm joints, levelled with a board. Lay outlines first, then fill the background in rows that follow them: the flow of the rows (the andamento) carries the eye.

The indirect (reverse) method (for workshop work and walls). Draw the design mirror-reversed on strong paper. Glue the tesserae face down on the paper with a water-soluble paste of flour or gum arabic (Glues and Adhesives). Cut the paper into sections of about 30 × 30 cm, numbered. On site, press each section paper-side up into a fresh mortar bed, and beat it level with a board. After an hour, wet the paper, peel it off, and correct any stray pieces. The face comes out perfectly flat.

Grout the finished mosaic as for tiles. Use lime putty and marble dust for fine work, or cement grout for floors.

Terrazzo

Terrazzo is a floor of marble chips set in cement and ground smooth. It wears like stone, can be laid in any pattern of colours, and uses up quarry waste (Quarrying and Cutting Stone).

  1. The underbed. Lay 1 cement : 4 sand, 3–5 cm thick, on a concrete slab, level or to the needed fall. Rough its surface.
  2. Divider strips. While the underbed is still soft, press in strips of brass, zinc or hard glass 3–4 cm deep (Zinc and Brass), standing up along the lines of the pattern. Space them no more than 1–1.5 m apart. They control cracking and separate the colours.
  3. The topping. Mix 1 part cement to 2–2½ parts marble chips (5–15 mm, washed), by volume, with only enough water to make a stiff mix. Add earth or metal-oxide pigments for coloured cement. Spread it 15–20 mm thick, a little above the strips.
  4. Seed and roll. Scatter extra chips over the surface and press them in with a heavy roller or a trowel until cement paste rises up. The finished floor should show about 70% stone on its face.
  5. Cure under wet sacking for 4–7 days. Do not let it dry out.
  6. Rough grind. Grind the floor wet with coarse abrasive stones or carborundum blocks (Abrasives and Grinding Stones) until all the strips and the chips are exposed and flat. By hand, use a heavy block on a long handle (with a weight on it) pushed back and forth, or a weighted stone dragged in circles. By machine, use a disc grinder. Wash off the slurry.
  7. Grout the pinholes. Rub a cement paste of the same colour over the whole floor to fill the holes, and cure it for 2–3 days.
  8. Fine grind and polish. Grind with progressively finer stones until it is smooth. Then polish with fine pumice or tin oxide on felt, finishing with wax.

Terrazzo can also be cast as tiles 30–40 cm square and 2.5–3 cm thick in steel moulds, ground on a bench, and laid like stone.

How to tell it worked

  • Tap test. Drag a coin over the cured floor: a dull click is good, a hollow sound means a void; reset that tile before it cracks.
  • Flatness. No lip (one tile edge above the next) over 1 mm under a straightedge; low window light shows them up.
  • Joints straight, even and full. Showers pass the flood test and stay dry below. Terrazzo shows evenly spread chips and no hollows by the strips.

Note Troubleshooting. Tiles drummy or loose → bed not full, paste skinned over before the tile was laid, or base dusty. Spread smaller areas, butter the backs, damp the base. Tiles crack in a line → the base below cracked or moved. Bridge cracks in the base, and add movement joints over joints in the slab. Tiles lift and tent up in a ridge → no gap at walls, or no movement joints. Cut out a row and leave the gaps. Grout cracks or powders → mixed too wet, or dried too fast. Rake out, regrout, and keep damp. White bloom on tiles and grout (efflorescence) → salts carried out by water. Brush off dry and wash with weak vinegar; stop the source of the damp. Wall tiles slide down → mortar too wet, too many rows at once, or no batten. Water stains below a shower → membrane holed, not turned up the walls, or the drain has no weep holes. Strip and retank; nothing else works.

Dangers

Danger Silica dust. Cutting, grinding and sawing tiles, stone and concrete dry fills the air with fine dust that scars the lungs (silicosis) over the years, and it cannot be cured. Always cut and grind wet, sweep up wet, and cover your nose and mouth with a damp cloth mask or better (Mining and Tunnelling).

  • Cement burns. Wet cement is strongly alkaline (Acids, Bases and Testing). Kneeling in it or leaving it on the skin causes deep, slow burns that are not felt until hours later. Wear gloves and knee pads, and wash it off with plenty of water. If it gets in your eyes, rinse them with clean water for 15 minutes.
  • Flying chips. Snapping tiles and cutting tesserae throws sharp chips. Protect your eyes with glass spectacles or a fine mesh shield.
  • Lead sheet for showers is poisonous to cut and handle carelessly. Wash your hands and don't eat while working (Lead).
  • Knees and backs. Floor tiling ruins knees. Use a thick pad and stand up every half hour.

What this unlocks

Tiled floors and walls make Toilets, Sinks, Baths and Showers, kitchens, dairies (Dairy and Cheese), slaughterhouses (Butchery and Meat) and operating rooms (Basic Surgery, Running a Hospital) washable and clean. Tiled stoves and masonry heaters (Chimneys, Stoves and Heating) store and radiate heat. Mosaic and terrazzo give public buildings, stations and schools floors that last centuries. Glazed tiles with painted designs (Glazes), encaustic tiles with coloured clay patterns pressed in, and cast cement tiles all use the same laying methods.

How it was first done

Glazed bricks and tiles decorated the walls of Mesopotamian and Egyptian buildings by the 2nd millennium BC; the blue-glazed Ishtar Gate of Babylon dates from about 575 BC. The earliest known pebble mosaics come from Gordion in Anatolia in about the 8th century BC, and the Greeks at Pella, in Macedonia, made superb pebble mosaics with lead strips for outlines in the 4th century BC. The Romans developed cut tesserae and laid them by the million, in fine pictures and plain floors alike, across their empire. Byzantine builders covered church domes with gold and coloured glass tesserae. In Morocco and Spain, zellige craftsmen chipped glazed tiles into interlocking geometric shapes from about the 10th century onward. Painted tin-glazed tiles spread from Spain and Italy to Delft in the Netherlands in the 1600s. In England, Herbert Minton revived machine-pressed encaustic floor tiles in the 1840s. Terrazzo grew from Venetian workers' habit of setting marble offcuts in lime floors, probably by the 1500s. Italian craftsmen carried it abroad in the late 1800s, and metal divider strips and electric grinding machines made it a common floor in the 1920s.