◆ Rebuild

Part 3 · Metals

Steel in Quantity

How to make steel by the tonne instead of the kilogram — melting it in crucibles, blowing air through molten cast iron in a Bessemer converter, and cooking it slowly in an open-hearth furnace — and how to remove phosphorus and judge the carbon without a laboratory.

Difficulty
●●●●●
Time
Weeks to build a crucible furnace and make pots; a season or more to build a converter or open hearth; a few hours per melt
Steps from zero
20 prerequisites →

You need first

The Blast Furnace and Cast IronFirebrick and RefractoriesSteel

This unlocks

Reinforced ConcreteSteel Frames and Tall BuildingsAlloy and Stainless SteelsRailways
The full path from nothing — 20 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. The Kiln
  10. Hides and Leather
  11. Bricks
  12. The Wheel and Axle
  13. Firebrick and Refractories
  14. Bellows
  15. Gears
  16. Iron (the Bloomery)
  17. The Waterwheel
  18. The Blast Furnace and Cast Iron
  19. Blacksmithing
  20. Steel
  21. Steel in Quantity

Do them roughly in this order. See it on the tech tree →

Why it matters

The methods in Steel — sorting steely pieces from blooms, carburising bars in a box, welding them into shear steel — give you kilograms of steel a week. That is enough for knives, axes and Files and Saws. It is not enough for rails, boilers, ship plates, bridges, wire rope, machine frames or the thousands of Screws, Nuts and Bolts an industry eats.

Before 1856 steel cost several times as much as wrought iron. Within forty years the converter and the open hearth made it the cheapest strong material on Earth. Steel in quantity is what makes Railways, Steamships, Steel Frames and Tall Buildings, Reinforced Concrete and Machine Tools possible.

This chapter covers three routes, smallest first:

  1. Crucible steel — melting steel in sealed clay pots. Small and slow, but within reach of a village with good fireclay and coke.
  2. The Bessemer converter — blowing air through molten The Blast Furnace and Cast Iron for 15–20 minutes. Needs a working blast furnace and a powerful blowing engine.
  3. The open-hearth furnace — a shallow bath of iron and scrap held molten for 8–12 hours by preheated gas. Slow, controllable, and able to use scrap.

Be honest about scale: the crucible is a workshop job; the converter and open hearth need a town with a Coal and Coke mine, a blast furnace and dozens of skilled people.

How it works

Removing carbon instead of adding it

Bloomery iron has almost no carbon; to make steel you must add carbon (see Steel). The blast furnace gives the opposite: liquid cast iron with 3.5–4.5% carbon plus some silicon, manganese, phosphorus and sulfur. To turn it into steel you must remove most of that carbon, down to 0.1–1%.

Carbon is removed by oxygen. Oxygen from air, or from iron ore (iron oxide) thrown into the bath, joins the carbon to make carbon monoxide gas, which bubbles out and burns at the mouth of the vessel. Silicon and manganese are burned out too, into the slag. The trick is to stop at the right carbon, and to keep the metal liquid while you do it: as carbon falls, the melting point of the metal rises from about 1,150 °C (cast iron) to about 1,500 °C (mild steel). The bath must get hotter as it gets purer.

Where the heat comes from

The crucible is heated by coke packed round the pots. The Bessemer converter burns no fuel at all: silicon and carbon burning inside the iron release so much heat that a blast of cold air makes the metal hotter. The open hearth burns gas, with the air and gas preheated by the furnace's own exhaust so that the flame reaches about 1,700 °C.

The problem of phosphorus and sulfur

  • Phosphorus makes steel cold-short: brittle at ordinary temperatures, so a rail snaps on a frosty morning. Above about 0.1% it is ruinous.
  • Sulfur makes steel hot-short: it cracks and crumbles when you forge or roll it red-hot.

In a furnace lined with acid refractory (silica, sand or ordinary fireclay), the slag is rich in silica, and phosphorus cannot be taken out of the metal. The cure, found in 1878, is a basic lining — burnt dolomite or magnesite instead of sand — and a slag rich in lime. Lime grabs the oxidised phosphorus and holds it in the slag. That slag, ground fine, is a valuable phosphate fertiliser ("basic slag", see Chemical Fertilisers). Manganese cures sulfur: it ties it up in harmless specks.

Killing the steel

Steel freshly blown or melted is full of dissolved oxygen. When it solidifies in the mould, the oxygen reacts with carbon and the ingot fizzes and fills with blowholes. Adding a deoxidiser just before pouring — manganese (as spiegeleisen, a manganese-rich pig iron), silicon, or later aluminium — removes the oxygen. Steel that lies quietly in the mould and does not bubble is called killed.

What you need

Item Crucible steel Bessemer Open hearth
Raw iron Blister steel, bloom iron + charcoal, or broken cast iron + bar iron Molten pig iron, 1–1.8% silicon, under 0.1% phosphorus (acid) Pig iron and steel scrap in any mixture
Batch size 10–30 kg per pot; 2–12 pots per furnace At least 1 tonne; normally 5–25 10–100 tonnes
Fuel Coke (about 3 kg per kg of steel), or charcoal with bellows None Producer gas from coal (see Biogas and Wood Gas and Gas Engines and Producer Gas for gas producers)
Air Natural draught from a 10–12 m chimney Blowing engine: about 1.5–2 bar, 200–400 m³ a minute for a 10-tonne blow Chimney draught
Refractories Fireclay + graphite crucibles; firebrick furnace Silica (ganister) or burnt dolomite lining Silica brick roof; sand or dolomite hearth
Additions Charcoal powder, a little glass or slag cover Spiegeleisen or ferromanganese Iron ore, limestone, spiegeleisen
People 2–4 10–30 10–30

See Firebrick and Refractories for firebrick and crucible clays, Coal and Coke for coke, The Blast Furnace and Cast Iron for the blast furnace and cupola, and Bellows to Air Compressors for blowing engines.

Where to find it

  • Fireclay — the grey-white, low-iron clay found under coal seams (the "seat earth" in which the coal plants grew). It stays solid far above the melting point of iron. See Firebrick and Refractories.
  • Graphite — soft, greasy, black-grey mineral that marks paper, found in marble and schist. In crucible clay it makes pots that survive sudden heat and are not wetted by steel.
  • Dolomite — looks like limestone but fizzes only weakly in cold vinegar (strongly when powdered or hot). Burned like lime (see Lime) but hotter, about 1,500 °C, it becomes a hard, basic refractory.
  • Quartz and ganister (a very pure, fine-grained sandstone with fireclay between the grains) make acid linings.
  • Limestone for basic slags — see Lime.
  • Iron ore for the open hearth — use rich, lumpy hematite or roasted ore (see Finding and Identifying Ores).

Method 1: Crucible steel

This is Benjamin Huntsman's Sheffield method, and the one to try first. It makes clean, even, slag-free steel for springs, razors and the cutting tools of Machine Tools.

Cover slablifted to see in Cruciblesfireclay + graphite,10–30 kg each Cokefist-sized, packedround the pots Firebrickand grate bars air from the cellar ash pit Molten steel1,550–1,600 °C,white and still when ready Flue Chimney10–12 m tall;its draught isthe only bellows Melting holeabout 50 × 50 cm,90 cm deep, floor level (continues upward)
Fig. 1 The crucible melting hole in cross-section. Pots stand on a stand in a firebrick pit filled with coke; a tall chimney pulls air up through the grate. The melter lifts a pot out through the top with long tongs.

The melting hole

  1. Dig and line the pit. Each "hole" is a firebrick-lined box about 50 × 50 cm and 90 cm deep, sunk so its top is level with the workshop floor. Under it is a cellar (the ash pit) where air comes in through an iron or clay bar grate.
  2. Flue and chimney. A flue 20 × 25 cm leaves the side of the hole near the top and runs to a chimney at least 10–12 m tall. The chimney is the bellows: a tall, warm chimney pulls air up through the grate hard enough to reach 1,600 °C. With a shorter chimney you need a powered blast at the ash pit.
  3. Cover. A firebrick slab in an iron frame closes the top. Lifting it shows you the inside.

The crucibles

  1. Mix fireclay with about one-third crushed old crucible (grog) and, if you have it, a third fine graphite. Huntsman's pots were plain fireclay; graphite pots came later and last longer.
  2. Tread it barefoot for an hour or more until smooth and free of air.
  3. Mould pots about 45 cm tall and 15–20 cm across inside, with walls 2.5–3 cm thick, in a wooden flask with a plug. Make a lid of the same clay.
  4. Dry them for at least two weeks in a warm room, then anneal (pre-fire) them to red heat just before use. A damp pot will crack the moment it meets the fire.

A plain clay pot lasts only 2–3 melts in one day; a graphite pot can last 10 or more.

The melt

  1. Charge each pot with 10–30 kg of broken blister or shear steel and a handful of charcoal powder. (Clean bar iron with 1–2% of its weight of charcoal also works; it carburises as it melts.) Put the lid on.
  2. Set the pots two to a hole on a firebrick stand (a "cheese") so they sit in the hottest part, and pack coke around and over them in pieces the size of a fist.
  3. Fire. Replenish the coke every 30–60 minutes. After 3–4 hours the charge should be melted.
  4. Check. Lift the lid with a rod. Look in: the metal should be white-hot, too bright to look at for long, and still. If you see sticky lumps or a crust, it is not ready.
  5. Kill it. Leave it in the fire another 30–60 minutes after it is melted. During this time it stops bubbling and goes quiet. This "killing" lets gases out and gives sound, blowhole-free ingots.
  6. Pull and teem. The puller-out, with wet sacking round his legs, lifts the pot out with long tongs. The teemer skims off the slag with a rod and pours the steel in a thin, steady stream into a split iron ingot mould that has been warmed and coated inside with a wash of clay or soot. Pour into the middle of the mould without touching the sides.
  7. Recharge the hot pot at once and put it back.

Crucible steel without coke

The Indian and Sri Lankan wootz makers melted in charcoal with bellows. Small crucibles (0.5–1 kg each) set in rows in a charcoal furnace with a strong forced blast reach melting heat in 6–8 hours. The output is tiny, but it is real cast steel.

Method 2: The Bessemer converter

Only attempt this once you have a blast furnace (see The Blast Furnace and Cast Iron) that can deliver at least a tonne of molten pig iron at a time, and a blowing engine driven by a The Steam Engine or Water Turbines and Hydroelectric Power. Smaller converters lose heat too quickly: below about half a tonne the metal freezes before the blow is finished.

Flame at the mouthread it to judge the blow (below) Steel or iron shell Lining, 25–40 cmganister (acid) or burnt dolomite (basic) Molten pig iron1–25 tonnes; never fill above thelevel of the trunnions Air bubblesburn out silicon, then carbon Trunnionthe vessel tilts to fill and pour Tuyeres and wind boxblast at 1.5–2 bar from the blowing engine 1. Silicon burns 3–5 min: short red-yellow flame and sparks 2. The carbon boil 10–12 min: long, roaring white flame, 5–10 m high 3. The drop flame shortens and fades: carbon gone, turn down now
Fig. 2 The Bessemer converter. Air from the blowing engine enters a wind box under the bottom and bubbles up through 25 or more holes in the tuyeres. The vessel tilts on its trunnions to take in iron and pour out steel.

The vessel

  • A pear-shaped shell of riveted iron or steel plate, about 2–2.5 m across and 4–5 m tall for a 5-tonne charge, hung on two trunnions (axles) so it can be tipped by a geared crank or hydraulic ram.
  • Lining 25–40 cm thick: rammed ganister (acid), or crushed burnt dolomite mixed with hot tar, rammed and baked (basic).
  • Bottom: a separate, replaceable plug holding a dozen or more fireclay tuyeres, each pierced with 8–12 holes of about 1 cm. Under it, an iron wind box that takes the blast. Bottoms wear out fastest — in 15–25 blows for a basic bottom — so make spares.

The blow

  1. Heat the lining with a coke fire until it glows bright red inside. Tip out the fire.
  2. Tip the converter onto its side so the tuyeres are above the level the iron will reach, and pour in the molten pig iron from a ladle.
  3. Turn on the blast, then raise the converter upright. The air must already be flowing before the iron covers the tuyeres, or the iron runs down into them and freezes.
  4. Watch the mouth. This is how the blowers judged it before anyone had instruments:
    • First 3–5 minutes: a short, reddish-yellow flame with showers of sparks. Silicon and manganese are burning.
    • Then the "boil": the carbon begins to burn. A long, roaring, dazzling white flame 5–10 m tall pours from the mouth, and the vessel shakes. This lasts 10–12 minutes.
    • The drop: quite suddenly, the flame shortens, thins and goes pale, transparent and wavering. The carbon is gone (under 0.1%).
  5. Turn down the converter at the drop and shut off the blast.
  6. Add spiegeleisen. Pour in 5–10% of the charge weight of melted spiegeleisen (pig iron with about 15–20% manganese and 4–5% carbon). It removes dissolved oxygen, fixes the sulfur, and puts back just enough carbon. Varying the amount sets the final carbon.
  7. Pour into a ladle and teem into ingot moulds.

A full blow takes 15–20 minutes. Its weakness is that it is over before you can test anything, and the air leaves nitrogen in the steel, which makes it slightly brittle with age.

The basic (Thomas) converter

With a dolomite lining you add burnt lime, about 12–18% of the iron's weight, to the converter before charging. The blow goes as above, but after the drop you keep blowing for another 3–5 minutes. This "after-blow" burns the phosphorus out into the lime, and the burning phosphorus supplies heat in place of silicon. The pig iron for this process must actually be high in phosphorus, about 1.8–2.5%, or the after-blow does not make enough heat. Pour off the thick slag before adding spiegeleisen, or the phosphorus goes back into the metal.

Method 3: The open-hearth furnace

The open hearth (also called Siemens–Martin) is slower but gives you control. You can take samples, test them and correct the bath before you pour, and you can melt scrap — the most useful property of all once a society has old rails, boilers and machines lying about.

Silica-brick roofflame about 1,700 °C under it Bath of iron and scrap30–60 cm deep, 10–100 t Flamehot gas and air meet at theport and burn across the bath Gas Air Checker bricks (regenerators) left pair: already hot, they preheat incoming air and gas to about 1,100 °C right pair: soaking up heat from the exhaust Reversing valves swap the flow every 20–30 min cold air in producer gas in to chimney
Fig. 3 The open-hearth furnace. Gas and air are preheated in hot checker-brick chambers before they meet over the bath. Every 20–30 minutes the flow is reversed, so that the exhaust reheats the chambers that have just cooled.

How it is built

  • A long, shallow hearth — a basin 30–60 cm deep — of rammed sand (acid) or burnt dolomite (basic), under a low arched roof of silica brick, which keeps its strength almost to its melting point.
  • At each end, ports that bring in gas and air.
  • Under each end, two brick chambers filled with a loose lattice of firebricks: the checkers or regenerators, one for air and one for gas.
  • Reversing valves that send the cold air and gas up through one end's checkers while the flame's exhaust goes down through the other end's checkers to the chimney.

The hot exhaust heats one pair of checkers to about 1,200 °C. When the flow is reversed, incoming air and gas pass through those hot bricks and are preheated almost to the same heat. Their flame is then hot enough to keep steel liquid. Reverse every 20–30 minutes. The gas is made in a gas producer: a deep bed of coal or charcoal burned with too little air and some steam, making carbon monoxide and hydrogen.

A heat

  1. Charge limestone (on a basic hearth), then scrap, then pig iron, through doors in the front wall, with long-handled peels or a charging machine. A common mix is half pig iron, half scrap.
  2. Melt down — 3–5 hours.
  3. Work the bath. Add lumps of rich iron ore to supply oxygen. The bath boils as carbon monoxide bubbles out. This "ore boil" takes 2–6 hours.
  4. Sample every 20–30 minutes: dip out a spoonful, pour a small test ingot, and test it (below).
  5. Finish when the carbon is right. Add ferromanganese or spiegeleisen to the bath or to the ladle, then open the taphole at the back and let the steel run into a ladle.

A full heat takes 8–12 hours.

Controlling and testing the carbon

You need to know the carbon before the steel is poured. With no laboratory:

  • The fracture test. Pour a small test ingot (about 3 × 3 × 15 cm) from a spoon, cool it in water, nick it and break it. Sheffield melters graded steel by eye from this fracture: high-carbon steel breaks with a fine, close, silvery grain; low-carbon steel with a coarse, bright, crystalline one; very soft steel bends instead of breaking. Keep labelled samples of known steels to compare with.
  • The spark test on a grindstone — see Steel.
  • The forge test. Forge the sample out flat and quench it. It should harden (high carbon) or bend double cold without cracking (mild steel), as wanted.
  • Watching the flame in the converter; watching the boil in the open hearth — a vigorous boil means plenty of carbon left.

Later, chemists matched samples by colour: the steel is dissolved in nitric acid (see Nitric Acid) and the brown colour of the solution compared against that of standard steels — the darker, the more carbon.

How to tell it worked

  • The ingot lies quiet in the mould and shrinks into a slight hollow at the top (the pipe). An ingot that rises and spits was not killed.
  • It forges. Steel that cracks at red heat is hot-short (too much sulfur — add more manganese next time). Steel that is fine hot but snaps cold is cold-short (phosphorus — use better ore or a basic lining).
  • Bend test. A strip of mild steel 6 mm thick should bend flat back on itself cold without cracking.
  • Hardening test. Tool steel should harden fully in water and break with a fine silver grain.

Note Troubleshooting. Crucible cracked in the fire → damp or not annealed; or set in cold and heated too fast. Dry for longer and warm pots before charging. Metal never melted fully → chimney draught too weak, or coke too small or wet. Use larger, hard coke and a taller or hotter chimney; clean the grate. Ingots full of holes → not killed long enough, or no deoxidiser. Give crucibles 30–60 minutes more; add spiegeleisen in the converter. Converter metal froze ("skulled") → pig iron too low in silicon, charge too small, or lining not preheated. Use iron with 1–1.8% silicon and heat the lining well. Steel brittle when cold → phosphorus. Use phosphorus-free ore, or go to a basic lining and lime slag. Basic lining crumbled to dust → burnt dolomite takes up water from the air and falls apart. Store it dry, mix it with tar, and use it within days.

Dangers

Danger Molten steel and water. Steel at 1,600 °C meeting water — a damp mould, a wet ladle, a puddle, damp lining — turns the water to steam in an instant and throws liquid metal across the shop. Every mould, ladle, tool and lining must be dry and warmed before metal touches it. Pour over dry sand floors.

Danger Converter and ladle spills. A converter holds tonnes of liquid metal. If the blast fails while it is upright, metal runs into the tuyeres and wind box. If the tilting gear fails, it pours where it points. Keep the area in front of the mouth clear of people at all times, and design the tilting gear so it fails safe.

Danger Carbon monoxide. Gas producers, open hearths and converters make large amounts of CO. Gas mains leak; a man walking into a pocket of producer gas collapses within a few breaths. Carbon monoxide has no colour or smell, and a lit candle does not warn of it (CO is a fuel, not a lack of oxygen); a caged small bird, which collapses first, is the old warning. Work only in well-ventilated buildings and never enter a flue or gas main without the gas shut off and the space aired.

  • Eyes. The light of white-hot steel and the converter flame damages the eyes. Look through dark blue or dark green glass.
  • Radiant heat. Teemers and pullers-out wore wet sacking and wooden-soled clogs. Heat stroke is a real risk: drink water and rotate the work.
  • Collapsing roofs. Open-hearth roofs eventually melt and fall in. Inspect them between heats.

What this unlocks

Cheap steel is the material of the industrial age: rails for Railways, plates for Steamships and boilers, wire for power lines, fences and Springs, beams for Steel Frames and Tall Buildings and Reinforced Concrete, and stock for Machine Tools and Precision and Interchangeable Parts. Rolling it into plate and sheet is covered in Sheet Metal and Rolling. The next step in steelmaking is the The Electric Arc Furnace, which melts scrap with electricity and makes the high-quality Alloy and Stainless Steels.

How it was first done

Benjamin Huntsman, a clockmaker in Doncaster and then Sheffield, England, wanted better steel for clock springs. Around 1740–1742 he succeeded in melting blister steel in clay crucibles in a coke fire, and Sheffield crucible steel became famous worldwide for a century and a half. Melted steel had been made long before in India, Sri Lanka and Central Asia as wootz.

In 1856 Henry Bessemer in England announced his process of blowing air through molten pig iron; the American William Kelly had experimented with the same idea earlier. At first it failed for most ironmasters, because their iron contained phosphorus. Robert Mushet showed that adding spiegeleisen afterwards made it work reliably. Göran Fredrik Göransson in Sweden, using phosphorus-free Swedish iron, made the process practical in 1858. In 1878 two cousins in Wales, Sidney Gilchrist Thomas and Percy Gilchrist, solved the phosphorus problem with a basic lining of dolomite, opening the phosphorus-rich ores of Lorraine and Germany to steelmaking.

Friedrich and William Siemens patented the regenerative furnace from 1856, and in 1864–1865 Pierre-Émile Martin in France used it to make steel on an open hearth. By the early 20th century the open hearth made most of the world's steel, until oxygen converters and electric furnaces replaced it after the 1950s.