Needles and Pins

How a workshop turns coils of steel and brass wire into thousands of sewing needles, pins and fish hooks a day — cutting, straightening, pointing, stamping and piercing eyes, heading pins, hardening, tempering and scouring — and why splitting the work into many small jobs made these tiny things cheap enough for everyone.

Difficulty
●●●●●
Time
An afternoon to make a dozen needles by hand; a few weeks to set up a small workshop making thousands a day
Steps from zero
17 prerequisites →

You need first

Iron and Brass Wire

This unlocks

—

Objects made here

sewing needlepinfish hook
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Iron (the Bloomery)
  13. Copper Smelting
  14. Blacksmithing
  15. Steel
  16. Copper Wire
  17. Iron and Brass Wire
  18. Needles and Pins

Do them roughly in this order. See it on the tech tree →

Why it matters

A steel needle is one of the smallest things in this book and one of the most used. Every garment, sail, tent, harness, book and mattress is sewn (Sewing, Needles and Thread, Making Clothes, Bookbinding, Mattresses and Upholstery). A bone needle works, but it is thick, breaks, and takes hours to make. A good steel needle is thinner than a bone needle's eye, lasts for years, and — made the right way — costs almost nothing.

Pins hold cloth for cutting and sewing, fasten papers and clothing, and mount insects and specimens. Fish hooks of hardened steel catch more fish than bone hooks and hold them better (Fishing). Knitting needles, sail needles, surgical needles (Basic Surgery), card teeth for combing wool (Textile Machinery) and the needles of the The Sewing Machine all come from the same skills.

This chapter is also about how to make things. One person doing every step makes perhaps a few dozen needles a day. Ten people, each doing one step with the right jig, make tens of thousands. That lesson — the division of labour — applies to almost everything else in a growing settlement (Precision and Interchangeable Parts).

How it works

A needle must be three things at once:

  1. Hard and springy, so it does not bend or blunt. That means good Steel, hardened by quenching and then tempered so it bends a little and springs back instead of snapping.
  2. Smooth, so it slips through cloth without dragging or cutting the thread. That means grinding, then hours of tumbling in grit and oil, then polishing.
  3. Shaped exactly: a fine round point, a slightly flattened head, and an eye with rounded edges that do not cut the thread.

The trick that makes needles cheap is to work on hundreds at once: cut wire to the length of two needles, straighten them in a bundle, point both ends in one go on a fast grindstone, stamp and pierce two eyes in the middle, then thread the pairs onto two fine wires and snap them apart. Every step handles a fan, a bundle, a tray or a bag of needles, never one at a time.

Pins are simpler: soft brass wire, cut, pointed and headed. They need no hardening, but brass tarnishes, so they are coated with tin.

What you need

Item Notes
Steel wire, 0.5–1.2 mm Medium-carbon steel (0.6–0.8% carbon), drawn soft (Iron and Brass Wire). 1 kg makes about 5,000 needles of 0.8 × 40 mm
Brass wire, 0.6–0.8 mm For pins (Iron and Brass Wire, Zinc and Brass)
Shears A heavy pair fixed to the bench, with a stop to set the length
Two iron rings 8–10 cm across, to hold a bundle of wire for straightening
Smooth iron plate and a curved iron bar For rolling bundles straight
Grindstone 30–60 cm across, fine sandstone, turned fast — by a treadle, a crank or a water wheel (Abrasives and Grinding Stones, The Waterwheel)
Hardened steel die and punches For stamping and piercing eyes; a drop-hammer or a hand screw press makes this far faster (Screws, Nuts and Bolts)
Fine files For burrs and heads (Files and Saws)
Iron tray and charcoal fire For hardening
Strong canvas or leather bags, rollers or a tumbling barrel For scouring
Emery or fine sand, oil, soft soap Scouring and polishing grit (Abrasives and Grinding Stones, Soap)
Tin and cream of tartar For whitening pins (Tin and Pewter; cream of tartar is the crust from wine barrels, Beer, Wine and Cider)

Method 1: Sewing needles in quantity

1 Cutdouble lengths 85 mm = two needles 2 Straighten, pointboth ends at once,50–60 wires in a fan 3 Stamp, piercetwo eyes in the middle(drawn enlarged) 4 Spitthread two fine wiresthrough all the eyes 5 Snap apartbend the comb in a vice;file all heads at once 6 Hardencherry red, about 800 °C,tipped into oil 7 Temperwarm until bright steelturns this colour straw240 brown260 purple280 blue300 needleshooks°C 8 Scourrolled in canvas with emery,oil and soap, for days board rolled back and forth 9 Finishburnish eyes, sharpen, sort, pack dryfinished, about 40 mm long
Fig. 1 Making needles two at a time. Wire cut to double length is straightened and pointed at both ends, stamped and pierced with two eyes in the middle, spitted on two fine wires and snapped apart; then the heads are filed, and the needles hardened, tempered and scoured.

For a single needle made at the bench, see Sewing, Needles and Thread. This method is the workshop version. The sizes below are for a general sewing needle 40 mm long and 0.8 mm thick; scale for others.

  1. Cut. Uncoil the soft wire and cut it on the shears into double lengths — here 85 mm (two needles plus a little waste). Set a stop on the shears so every piece is the same length.
  2. Straighten. Pack 3,000–5,000 pieces tightly inside two iron rings, one near each end, like a bundle of sticks. Heat the bundle to a dull red (about 650 °C) in the fire, put it on the iron plate, and roll it back and forth under the curved bar for a minute or two. The wires rub each other straight. Let it cool slowly; the wire stays soft.
  3. Point. This was the best-paid and deadliest job. The pointer takes 50–60 wires, spreads them in a fan between his fingers and thumbs, and holds their ends against a fast-turning grindstone, rolling them with his thumb so every wire turns as it grinds. A few seconds forms a round, tapered point 3–5 mm long on every wire in the fan. Turn the fan round and point the other ends. Grind wet if you possibly can (see Dangers).
  4. Stamp. In the middle of each double wire, stamp the two eyes' shapes with a hardened die: a press or a blow from a small drop-hammer flattens the middle slightly and marks two long grooves (the gutters, which let the thread lie flush) and two eye outlines, end to end.
  5. Pierce. Put the stamped wire in a second die and punch the two eyes right through with a pair of fine hardened punches. A good eye for a 0.8 mm needle is about 0.3 × 1.2 mm.
  6. Spit. A child's or beginner's job: thread a fine stiff wire (the spit) through all the first eyes of 50–100 double needles, and a second spit through all the second eyes. The needles now sit side by side like a comb.
  7. Break and file. Clamp the comb in a vice and bend it back and forth: the double needles snap apart in the middle, leaving two combs of single needles. File the rough broken ends of the whole comb at once until each head is round and smooth. Slide the needles off the spits.
  8. Harden. Spread the needles in a single layer on an iron tray, heat them in a charcoal fire to an even cherry red (about 800 °C), and tip them all at once into a pan of oil or water. They come out glass-hard and brittle (Steel).
  9. Temper. Roll the hardened needles on a hot iron plate, or warm them in a pan of hot sand, until a bright one turns from straw yellow to brown or purple (about 240–280 °C). Tip them off to cool at once. Now they bend slightly and spring back.
  10. Scour. Put 20,000–50,000 needles side by side in a strip of canvas with a mixture of emery powder, oil and soft soap, roll it into a tight sausage, tie it, and roll it under a heavy board, or in a turning barrel, for 8–10 hours. Wash the needles in hot soapy water, sieve them, and repeat with finer and finer grit five or six times over a week. This polishes the whole needle, rounds the eye edges and takes off the scale from hardening. Dry them in hot sawdust or bran to stop rust.
  11. Finish. Sort out bent and broken needles (roll them on a flat plate: bent ones wobble). Burnish the eyes by threading needles on a fine, roughened steel wire spinning fast, or with a fine countersink drill from each side. Give the points a last touch on a fine, fast stone.
  12. Store in folded black paper or waxed paper, dry. Steel needles rust in a damp week.

Other needles.

  • Sail and leather needles: 1.5–3 mm wire, 60–100 mm long, with a three-sided point filed or ground after pointing (Ropewalks and Sailcloth, Hides and Leather).
  • Knitting needles: 2–6 mm steel or brass wire, pointed and polished, not hardened (Knitting, Crochet and Netting).
  • Darning and bodkin needles: thicker wire, large eyes, blunt points.
  • Fine needles below 0.5 mm are too small to punch: drill the eye with a tiny flat drill turned by a bow (Drills and Boring), or form a split eye.

Method 2: Pins

Pins (enlarged) Fish hook (enlarged) Spun head (old way) two turns of fine wire slipped on and clamped by a blow in a small die Solid head (better) the blunt end upset by a cupped punch, like a rivet head Real pin: 25 mm long, 0.6–0.8 mm brass, whitened by boiling with tin Eye Shank Point filed, then resharpened Barb a sliver cut and lifted Bend round a peg Gape about 10 mm for 0.7–1 mm wire; tempered to dark blue
Fig. 2 A brass pin and a steel fish hook. The old pin had a separate coiled wire head clamped on; later pins had heads struck from the shank itself. The hook needs a sharp point, a barb lifted from the wire, a bend and an eye.

Adam Smith counted eighteen separate operations in an 18th-century pin workshop. The main ones:

  1. Draw brass wire to 0.6–0.8 mm and anneal it soft (Iron and Brass Wire).
  2. Straighten it by pulling it through a zigzag of 6–8 iron pegs set in a board — a straightening board. Pull 5–10 m at a time and cut it into long lengths.
  3. Cut into lengths of several pins at once, then into pin lengths: 25 mm for dressmaking pins.
  4. Point in fans on a fine grindstone, as for needles. Brass grinds easily; a second, finer wheel gives a sharp point.
  5. Head. Two ways:
    • Spun heads (the old way): wind fine brass wire, half the pin's thickness, tightly round a wire mandrel into a long coil; cut the coil into rings of two turns each; anneal them; slip one ring over the blunt end of each pin, and strike it once or twice in a small die with a falling weight worked by a pedal. The ring clamps onto the shank as a round head.
    • Solid heads (better): grip the pin in a clamp with 1 mm sticking out of the blunt end and strike the end with a cupped punch. The brass upsets (squashes) into a neat round head, just as a rivet head forms (Nails, Rivets and Wire Fasteners). Two blows: one to gather, one to shape.
  6. Whiten. Brass pins turn green and stain cloth. Clean them in weak acid or vinegar, rinse, then boil them for an hour or two in a copper pan with a solution of cream of tartar in water and layers of grain tin or tin shavings. A thin silvery film of tin coats each pin. Rinse, and tumble them in dry bran or sawdust to dry and polish.
  7. Paper. Stick them in rows through folded paper so they can be counted and sold.

Safety pins are a single piece of springy steel or brass wire, 0.8–1 mm, bent with a coil in the middle (the spring) and a sheet-metal cap at the head to guard the point. Harden steel ones a little after bending, or use hard-drawn brass (Springs).

Method 3: Fish hooks

Steel hooks are stronger and sharper than any bone hook (Fishing).

  1. Cut soft steel wire to length: for a hook with a 10 mm gap (the gape), 0.7–1 mm wire, about 35 mm long.
  2. Barb. Clamp the wire, and with a sharp chisel-edged knife held at a shallow angle, cut a sliver into the wire 3–5 mm from one end, lifting it outward without cutting it off. This raised sliver is the barb.
  3. Point. File or grind the end beyond the barb to a sharp, slender point. Sharpen it again after hardening.
  4. Bend. Bend the hook round a polished steel peg of the right diameter set in a board, with the barb on the inside.
  5. Form the eye or spade at the other end: bend a small loop round a thin pin, or hammer the end flat (a spade end) for whipping to the line.
  6. Harden and temper as for needles, but temper a little softer — to dark blue (about 300 °C) — so the hook flexes rather than snapping on a heavy fish.
  7. Protect. Coat the hooks with a thin film of oil varnish or black japan (linseed oil cooked with asphalt), or tin them like pins. Steel hooks left bright rust in a day of sea water.

The division of labour

In 1776 Adam Smith described a small pin workshop where ten people, each doing one or two operations, made about 48,000 pins a day — 4,800 each — while one person doing everything alone could hardly make twenty. The reasons hold for any small product:

  • Each worker becomes fast and skilful at one motion.
  • No time is lost changing tools and tasks.
  • Each step can have its own jig, die or machine, built for that one job — and once a step is mechanical, a machine can take it over.

Organise your workshop as a line: wire coils at one end, a cutter, a straightener, a pointer at the grindstone (on its own, out of the way, with the best ventilation and water), a stamper and piercer with a press, a filer, a hardener at the fire, the scouring barrels, and sorters and packers in good light. Keep each worker's batch in a counted box so you can see where work piles up.

How to tell it worked

  • Point: push the needle through two layers of tight cotton cloth held up loosely — a good needle slides through without a sound and without pushing the cloth ahead of it.
  • Eye: pull a fine thread back and forth through the eye 50 times. It must not fray or cut.
  • Temper: bend a needle about 20° between finger and thumb and let go. It should spring back straight. If it stays bent, it is too soft (temper less); if it snaps, too hard (temper more).
  • Finish: a scoured needle is evenly bright with no scale, and smooth under a fingernail.
  • Pins: push one through folded cloth 20 times; the head must not come off and the point must not curl.
  • Hooks: hang a weight on a hook: a hook with a 10 mm gape in 0.8 mm wire should hold a few kilograms without opening.

Note Troubleshooting. Needles snap after hardening, even with careful handling → not tempered, or wire too high in carbon. Temper to brown or purple. Needles bend and stay bent → too low in carbon (iron, not steel), not hot enough when quenched, or tempered too far. Check the wire with a spark test (Steel). Eyes crack when punched → the wire was work-hardened. Anneal the stamped blanks at dull red before piercing. Thread frays in the eye → eye edges sharp. Scour longer, or burnish the eyes. Needles rust in the packet → not dried properly after scouring, or stored damp. Dry in warm bran, pack in waxed paper. Pins come out patchy brass and tin → the brass was greasy or tarnished. Clean in weak acid first, and boil longer with fresh tin. Hooks open out on a fish → too soft or too thin. Use thicker wire or temper only to purple.

Dangers

Danger Pointer's lung. Dry-pointing on a fast grindstone fills the air in front of the grinder's face with steel dust and stone dust. In 19th-century needle towns, pointers commonly died of lung disease in their thirties. Grind wet — a trough of water under the stone, or a drip on its face — and put the grindstone where a draught or a hood carries the dust away from the face. Cover nose and mouth with a damp cloth. Change who points every few days. See Abrasives and Grinding Stones.

Danger Bursting grindstones. A fast-turning grindstone can break and throw heavy pieces with enough force to kill. Check every stone for cracks by tapping it (a sound stone rings; a cracked one clunks), never run it faster than its usual speed, and stand to the side when starting it. See Abrasives and Grinding Stones.

  • Points and splinters. Thousands of sharp points in a workshop will find hands and eyes. Handle needles in fans and bundles with the points away from you. Sweep the floor with a magnet on a stick for lost needles; children and animals swallow them.
  • Hot oil. Quenching trays of red-hot needles in oil can make the oil flare. Keep a lid ready to drop on it.
  • Swallowed pins. Never hold pins in the mouth.

What this unlocks

Fine steel needles for all Sewing, Needles and Thread, Making Clothes, Hides and Leather and sail work; the needle of the The Sewing Machine; card teeth for carding wool and cotton (Textile Machinery); hooks for Fishing; surgical needles (Basic Surgery, Wound Care and Antiseptics); pins for dressmaking, papers and pinned specimens (Cells, Life and Evolution). And the habit of breaking any job into simple steps with jigs and dies leads straight to Machine Tools and Precision and Interchangeable Parts.

How it was first done

Bronze and iron needles were common in the ancient world, and Roman needles look much like ours. Steel needles were being made in quantity in Islamic Spain and in Nuremberg by the late Middle Ages. In England, needle-making settled around Redditch in Worcestershire from the 1600s; by the 1800s it made most of the world's needles, using water-powered scouring mills and, from the early 1800s, presses for stamping and piercing eyes. The pointers' early deaths were notorious; a magnetic mask to catch steel dust was tried in Sheffield in the 1820s, and wet grinding and fans came in slowly.

English pin-making began in Gloucester in 1626. Adam Smith used a pin workshop to open The Wealth of Nations (1776). In the United States, Lemuel Wright patented a pin machine in 1824, and John Ireland Howe built a machine that made complete solid-headed pins in the 1830s. Walter Hunt patented the safety pin in New York in 1849. Redditch also made fish hooks; in Norway, the Mustad works at Gjøvik began machine-making hooks in the 1870s and grew to be the world's largest maker.

Source: content/entries/metals/needles-and-pins.md