Materials you can mould into any shape — buttons, insulators, combs, handles, records. Start with shellac from an insect and casein from milk; Bakelite, made from coal-tar phenol and formaldehyde, is the first fully synthetic plastic. Celluloid is described only in outline because it is so flammable.

Difficulty
●●●●●
Time
A day to make shellac moulding compound; weeks to harden casein in formaldehyde; minutes per pressing once the mould is hot
Steps from zero
13 prerequisites →

You need first

Nitric AcidDistillation

This unlocks

Composites: Fibreglass, Carbon Fibre and HoneycombPhotographic Film BasePetrochemicals and Modern PlasticsRayon and Nylon
The full path from nothing — 13 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. The Kiln
  6. Lime
  7. Lye and Potash
  8. Fermentation
  9. Glass
  10. Saltpeter
  11. Distillation
  12. Sulfuric Acid
  13. Nitric Acid
  14. Early Plastics

Do them roughly in this order. See it on the tech tree →

Why it matters

Wood, stone, metal and clay are shaped by cutting, beating or firing. A plastic is shaped by pressing it into a mould: once the mould is made, you can turn out a thousand identical buttons, knobs, switch covers or combs, each in a few minutes, each with every detail of the mould. That is a new kind of manufacturing.

Early plastics also filled real needs:

  • Electrical insulation. Switches, sockets, fuse holders, telephone and radio parts need a material that is rigid, mouldable and does not conduct. Shellac and then Bakelite made the electrical age practical (Wiring and Electrical Safety, The Telephone, Radio).
  • Substitutes for scarce natural materials — ivory, tortoiseshell and horn — for combs, handles, buttons and spectacle frames (Spectacles).
  • Sound recording and film — shellac gramophone records and celluloid photographic film (Recording Sound, Photography).

The good news: the two easiest plastics come from an insect and from milk, and need almost no chemistry. The bad news: the most famous early plastic, celluloid, is made from a close relative of guncotton and burns almost explosively, so this chapter only outlines it.

How it works

Every plastic is made of long chain molecules (polymers) — thousands of small units linked end to end, like beads on a string. Long chains tangle together, which makes the material tough instead of crumbly. Two kinds matter:

  • Thermoplastics soften every time they are heated and harden when cooled, like wax. Their chains are separate and can slide past each other when warm. Shellac, gutta-percha, celluloid and horn are thermoplastics: you can reheat and reshape them, and scrap can be remelted. But they soften again in heat.
  • Thermosets set once and for ever. During heating, the chains form cross-links — bridges between chains — until the whole piece is one giant molecule. Then heat cannot soften it; it only chars. Bakelite, hard rubber (Rubber) and formaldehyde-hardened casein are thermosets. They are stiff, heat-resistant and do not dissolve.

Most early plastics were mostly filler: wood flour (very fine sawdust), slate or limestone dust, cotton fibre or mica, held together by a smaller amount of the plastic binder — like gravel held by cement in concrete (Mortar and Concrete). Filler makes the plastic cheaper, stiffer and less likely to crack.

RAW MATERIALPLASTICGOOD FOR Lac insect resinscraped from twigs Tree latexgutta-percha; rubber + sulfur Milk+ formaldehyde to harden Coal tar → phenolwood spirit → formaldehyde+ wood flour filler Cotton + nitric acid+ camphor Shellac compoundthermoplastic, easiest Gutta-percha, ebonitethermoplastic / thermoset Casein (Galalith)thermoset once hardened Bakelitethermoset; first fullysynthetic plastic Celluloidoutline only: very flammable Records, insulators,cases (keep cool) Cable insulation,battery boxes, combs Buttons, combs,handles (keep dry) Switches, sockets,telephones, radios,laminated boards Film, billiard ballsreplaced by safer plastics
Fig. 1 The early plastics and where they come from. Natural resins and gums come first; casein needs only milk and, for hardening, formaldehyde; Bakelite needs phenol from coal tar and formaldehyde from wood spirit; celluloid needs nitric acid and is the most dangerous.

What you need

For Materials Equipment
Shellac compound Shellac (or sticklac to make it), wood flour or slate dust, a little soot for black A heavy iron plate over a fire, a scraper, metal moulds, a press
Casein plastic 10 litres of skim milk gives about 250–300 g of dry casein; vinegar or rennet; formaldehyde solution for hardening Pots, cloth, a press, a mill or mortar, glass or glazed pots for hardening
Bakelite (outline) Phenol, formaldehyde solution, a little ammonia or acid, wood flour Glass or enamelled vessels, a steam-heated steel mould, a strong press
Moulds and press Cast iron, bronze or brass (Metal Casting) A screw press (Screws, Nuts and Bolts) or hydraulic press (Hydraulic Presses and Rams)

Where to find it

  • Lac is the resin secreted by tiny scale insects (Kerria lacca) that crowd on the twigs of certain trees in India, Thailand and southern China — palas (flame of the forest), kusum, ber (jujube), rain tree, pigeon pea and some figs. Infested twigs are encrusted with a hard, red-brown, bumpy resin up to 1 cm thick: this is sticklac. Lac can be farmed by tying infested twigs to new host trees.
  • Milk: from cows, goats, sheep or buffalo (Keeping Animals, Dairy and Cheese). Skim the cream off first: fat spoils casein plastic.
  • Horn: cattle, sheep and goat horn (Hunting and Trapping, Keeping Animals).
  • Gutta-percha: the latex of Palaquium trees in Malaysia and Indonesia; balata from South American trees — see Rubber.
  • Phenol: from distilling coal tar, the by-product of making coke and coal gas (Coal and Coke, Coal Tar Chemicals). Phenol is the "carbolic acid" of old disinfectants and smells like it.
  • Formaldehyde: made from methanol (wood spirit, Ether, Acetone and Solvents); see Methanol and Formaldehyde.

Method 1: Horn and shellac — natural thermoplastics

Horn. Before any plastic, horners pressed horn. Boil horn in water for an hour or two until it is leathery, slit it, open it flat, and press it between warm iron plates. Thin sheets can be pressed into simple moulds for buttons, spoons and combs, or split and scraped until they are translucent for lantern windows (Lamps and Candles).

Making shellac from sticklac.

  1. Scrape the resin off the twigs and crush it to grains.
  2. Wash it in several changes of water, rubbing well. The water turns deep red: that is lac dye, a good crimson dye for wool and silk — keep it (Dyes and Mordants). Washed and dried, the grains are seedlac.
  3. Melt and strain. Fill a long, narrow cloth bag with seedlac and hold it before a fire. As the lac melts it oozes through the cloth, leaving dirt and insect bodies inside; twist the bag to squeeze it out and scrape the melt onto a smooth, wet surface. Stretched thin while warm, it sets as glassy amber sheets, which you break into flakes. (Alternatively, dissolve seedlac in strong alcohol, let it settle, filter, and evaporate.)

Shellac moulding compound.

  1. Mix by weight about 1 part shellac with 1½–2 parts filler — fine slate or limestone dust for hard, smooth pieces (records, insulators), wood flour for lighter, tougher ones (cases, handles). A spoonful of soot gives black.
  2. Knead hot. Heat a thick iron plate until a drop of water flicked on it sizzles and boils away but does not skate around (about 110–130 °C). Work the mixture on it with a flat iron scraper until the shellac melts and wets every grain, forming a stiff, even dough.
  3. Roll it into sheets or cut it into pieces of a weighed size (see Moulding, below), and either mould at once or let them cool and reheat later.

Shellac pieces are hard, glossy and excellent insulators, but brittle and they soften above about 60–70 °C and dissolve in alcohol. Do not use them for anything that gets hot.

Method 2: Casein plastic (milk stone)

Casein is the main protein of milk — the part that forms the curd of cheese. Dried and pressed, then soaked in formaldehyde, it becomes a hard, horn-like plastic, the Galalith ("milk stone") that made billions of buttons.

  1. Curdle. Warm 10 litres of skim milk to about 35–40 °C — comfortably warm to a finger. Stir in vinegar a little at a time, about 80 ml per litre, until the milk separates into white curds and clear greenish whey. (Rennet, the calf-stomach extract used for cheese, gives a firmer curd that makes better plastic — see Dairy and Cheese.)
  2. Strain through a cloth. Wash the curd three or four times in clean warm water, squeezing it each time, to remove whey, acid and fat.
  3. Press and dry. Press out as much water as you can, crumble the curd, and dry it thoroughly in a warm airy place, until it is hard, dry granules. 10 litres give about 250–300 g.
  4. Grind the dry casein to a fine powder in a mortar or mill.
  5. Make the dough. Knead the powder with hot water — about 1 part water to 3 parts casein by weight — until it becomes a stiff, plastic dough. Colour it now with any dye or pigment (Pigments, Paints and Varnish).
  6. Shape. Press the warm dough into sheets 2–5 mm thick between greased boards, roll it into rods, or press it into moulds. Let the shapes firm up for a day.
  7. Harden. Lay the pieces in a glass or glazed pot of 4–5% formaldehyde solution (strong formalin diluted about eight times with water), cover tightly, and keep it outdoors or in a shed. Formaldehyde ties the casein chains together. This is slow: a few days for thin buttons, two to four weeks for a 3 mm sheet, months for thick blocks. Cut a test piece: hardened casein is the same colour right through; an unhardened core is paler and softer.
  8. Dry slowly. Air-dry the hardened pieces over several weeks, turning them and weighting sheets flat, or they warp and crack.
  9. Finish. Saw, drill, file, turn on the The Lathe and polish like horn. Hardened casein cannot be remoulded.

Casein plastic takes dye beautifully and feels like horn or ivory, but it absorbs water and swells — fine for buttons, knitting needles, combs, buckles, pens and handles, poor for anything left wet or for electrical parts in damp places.

Tip No formaldehyde yet? Unhardened casein dough, simply dried, makes hard but brittle beads, buttons and small ornaments. Keep them dry. The same casein mixed with slaked lime is casein glue (Glues and Adhesives).

Formaldehyde in outline. Methanol vapour mixed with air is passed over a coil of copper wire or gauze kept at a dull red heat; the copper helps the methanol give up hydrogen and become formaldehyde gas, which is absorbed in water to give formalin (up to about 37–40%). Formaldehyde is a poison and an irritant (see Dangers); this step needs Laboratory Glassware and outdoor work, and Methanol and Formaldehyde gives it in full.

Method 3: Bakelite (outline)

Bakelite is made by joining phenol and formaldehyde into a resin and then baking it hard under pressure. It was the first plastic made entirely from chemicals, not from a natural polymer.

  1. The resin. Phenol and formaldehyde solution are heated together with a small amount of a helper (catalyst): a little ammonia or alkali for a resol resin, a little acid for a novolac resin. The mixture turns cloudy, separates into a heavy, honey-like resin and water, and is boiled down until a sample sets brittle when cold.
  2. Moulding powder. The cooled, brittle resin is ground with about its own weight of wood flour, a little lubricant (wax or a metallic soap) and pigment (usually black or brown). Novolac resins also need a hardener added at this stage.
  3. Moulding. A weighed charge is pressed in a polished steel mould at about 150–170 °C for a few minutes under strong pressure. It first softens and flows to fill every corner, then cross-links and sets rigid in the mould. The pressure stops water vapour, given off as it sets, from blowing bubbles.
  4. Laminates. Paper or cotton cloth soaked in liquid resin, stacked and hot-pressed, makes hard, strong boards — panels and gears for electrical machines, and later the base boards of circuits.

Bakelite is hard, stiff, heat-resistant, does not burn easily, does not absorb water and is an excellent electrical insulator. It cannot be remelted. Its weakness is brittleness. The resin kettle, moulding powders and laminates are covered properly in Resins: Phenolic, Polyester and Epoxy.

Celluloid (history and outline only)

Celluloid is nitrocellulose — cotton or wood cellulose that has been treated with nitric acid (Nitric Acid) — kneaded with camphor (a fragrant crystal from the camphor laurel tree) and alcohol into a dough, pressed into blocks, sliced into sheets and seasoned for weeks. It moulds when warm, can be made clear, coloured or imitation tortoiseshell, and was used for billiard balls, collars, combs, toys and, above all, photographic and cinema film.

Nitrocellulose is a close relative of guncotton, an explosive. This book does not describe how to make it. Celluloid catches fire easily, burns very fast, cannot easily be put out (it carries its own oxygen) and gives off poisonous fumes; old celluloid film can even decompose and ignite by itself. Use the safer plastics in this chapter; for film, see the alternatives in Photography and the acetate safety film of Photographic Film Base.

Moulding

Screw pressor lever / hydraulic press Platen Upper half (force) Guide pinshalves always meet true Chargeweighed, 5–10% extra Heated platefire or steam Taper 1–2°so the piecepulls free Cavitypolished, greased THE PRESSED PIECE thin flash to trim off
Fig. 2 A compression mould in a press. A weighed charge goes into the heated lower half; the upper half (the force) is pressed down, the softened plastic fills the cavity, and a little excess squeezes out as a thin "flash" that is trimmed off afterwards.
  1. Make the mould in two halves of cast iron, bronze or brass (Metal Casting), with guide pins so the halves always meet in the same place. File and polish the cavity smooth: every scratch shows on every piece. Give every wall a slight taper — 1–2° — so the piece pulls out.
  2. Weigh the charge: a little more than the piece needs (5–10% extra). Too little and the corners do not fill; too much and the mould cannot close.
  3. Heat the mould. Shellac: water flicked on it sizzles but does not skate (110–130 °C). Bakelite: a pinch of sulfur on it melts and then just turns from yellow to dark red-brown (about 160 °C). Steam pipes or a gentle fire under a thick plate keep it even.
  4. Grease the cavity lightly with soap, wax or oil.
  5. Press. Load the charge, close the mould and press hard with a screw or lever press. Hold: shellac until the mould has cooled enough to set it (cool the mould with a wet cloth); Bakelite for 2–5 minutes hot.
  6. Open, eject, trim the flash with a file, and polish.

How to tell it worked

  • Shellac pieces are glossy, ring when tapped, show every detail of the mould, and do not crack when dropped on a wooden table from 30 cm.
  • Hardened casein cuts evenly to the core, does not soften in boiling water for a minute (unhardened casein turns leathery), and polishes to a horn-like shine.
  • Bakelite does not soften on a hot plate — it only chars if very hot — and does not dissolve in alcohol or acetone.
  • Insulation test. Put a piece between two wires connected to a battery and lamp or bell (The Battery). Nothing should light.

Note Troubleshooting. Shellac pieces crumbly → too little shellac, or it never fully melted. Use more shellac; knead hotter. Unfilled corners → charge too small, mould too cool, or not enough pressure. Bubbles or blisters → damp filler, or the mould was opened while gas was still forming. Dry the filler; hold pressure longer. Pieces stick in the mould → no taper, a rough cavity, or no grease. Casein warps and cracks → dried too fast. Dry slowly, weighted, in shade. Casein soft in the middle → not long enough in formaldehyde.

Dangers

Danger Phenol passes straight through skin. Strong phenol splashed over a large area, such as a whole arm, has killed people within hours (Coal Tar Chemicals). It numbs as it burns, so you may not feel how bad it is, and the skin turns white. Wear gloves and eye protection; wash any splash at once with large amounts of water for at least 15 minutes (soapy water or vegetable oil helps lift it). Its vapour also poisons.

Danger Celluloid and nitrocellulose burn violently and give off poisonous gases. Fires in stores of celluloid film have killed many people — 123 died in the Cleveland Clinic fire of 1929, started by nitrate X-ray film. Do not make it, and do not store old nitrate film in living spaces.

  • Formaldehyde stings the eyes, nose and lungs, causes skin allergies, and is linked to cancer with long exposure. Work outdoors or in a strong draught, keep hardening pots covered, and never use it indoors where people sleep. Its starting material, methanol, is a poison (Ether, Acetone and Solvents).
  • Nitric acid for celluloid: see Nitric Acid.
  • Hot moulds, presses and molten shellac burn. A screw press can crush fingers — keep hands out of the mould while closing it.
  • Dust. Wood flour and slate dust in the air harm the lungs; wet-grind or wear a cloth mask.

What this unlocks

How it was first done

Lac has been gathered in India for at least 3,000 years — as dye, as varnish and as sealing wax. Gutta-percha came to Europe in 1843 and was soon moulded into everything from furniture ornaments to golf balls; it insulated the first undersea telegraph cables in 1850–51. In 1854 Samuel Peck in the United States patented moulded "Union cases" for photographs, made of shellac and wood fibre, and from the 1890s Emile Berliner's gramophone records were pressed from shellac and slate dust.

Alexander Parkes showed "Parkesine", the first celluloid-type plastic, at the 1862 International Exhibition in London, but his company failed. In the United States the printer John Wesley Hyatt, chasing a prize for a substitute for ivory billiard balls, and his brother Isaiah patented celluloid in 1870. In 1897 Wilhelm Krische and Adolf Spitteler in Germany found that formaldehyde hardened casein, and Galalith went into production a few years later. August Wilhelm von Hofmann had made formaldehyde from methanol over hot platinum in 1867.

Adolf von Baeyer noticed the sticky resin from phenol and formaldehyde in 1872, but thought it useless. In 1907 the Belgian-American chemist Leo Baekeland in Yonkers, New York, found how to control the reaction and harden the resin under heat and pressure, and patented Bakelite in 1909, calling it "the material of a thousand uses". Within twenty years it was in every radio, telephone and car.

Source: content/entries/chemistry/early-plastics.md