Zircon and Zirconium

Zircon is a hard, heavy, glassy sand found with the black sands of beaches and rivers. It makes refractory bricks that molten glass cannot eat, foundry sand that steel cannot burn into, and the cheapest white opacifier for glazes and enamels; turned into zirconia, it makes crucibles for 2,000 °C, tough ceramics and gems. How to separate it, grind it and use it, how to make zirconia, and zirconium metal in outline.

Difficulty
●●●●●
Time
Days to concentrate zircon sand; a week for a batch of opacifier or bricks; weeks of chemistry for zirconia
Steps from zero
6 prerequisites →

You need first

Rocks and MineralsFirebrick and Refractories

This unlocks

—
The full path from nothing — 6 steps before this one
  1. Fire
  2. Rocks and Minerals
  3. Finding and Preparing Clay
  4. The Kiln
  5. Bricks
  6. Firebrick and Refractories
  7. Zircon and Zirconium

Do them roughly in this order. See it on the tech tree →

Why it matters

Molten glass slowly dissolves fireclay bricks (Firebrick and Refractories); a glass tank lined with them is eaten through in months and its glass is spoiled with stones and streaks. Steel poured into ordinary sand moulds fuses the sand onto the casting, which then takes hours of chipping. White glazes and enamels need tin oxide, and tin is rare and dear. One cheap mineral, picked from the same beach sands that give titanium (Titanium) and rare earths (Rare Earths, Cerium and Phosphors), solves all three: zircon.

From zircon you can also make zirconia (zirconium oxide). It melts at about 2,700 °C, hotter than almost any other oxide you can make, so a zirconia crucible holds molten platinum and special steels. Made with a few per cent of lime, magnesia or yttria, it becomes one of the toughest ceramics known: knives, pump seals, wire-drawing dies (Iron and Brass Wire), dental crowns. It coats the hottest parts of jet engines (Jet Engines), senses oxygen in engine exhaust, and when melted and grown into crystals makes the brilliant gem called cubic zirconia (Synthetic Gems). The metal itself is almost invisible to neutrons and resists acids, which makes it the tubing of nuclear fuel (Nuclear Energy (Overview)).

How it works

Zircon is zirconium silicate. Its grains are:

  • Heavy: about 4.6 times as heavy as water (quartz is 2.65), so it collects with the heavy minerals in moving water.
  • Hard: 7.5 on the scratch scale, harder than quartz.
  • Very stable: it hardly expands when heated, is not wetted by molten iron, steel, aluminium or glass, and resists acids. Above about 1,650 °C it slowly breaks up into zirconia and silica glass.
  • Very high in refractive index (it bends light strongly, about 1.95 against glass's 1.5). Tiny grains of it inside a glass scatter light, as fine bubbles do in foam, and the glass turns white and opaque.

Zirconia has a flaw: when it cools through about 1,000 °C (the change runs the other way near 1,170 °C on heating) its crystals change form and swell by 4–5 %. A pure zirconia pot shatters itself on cooling. Dissolving a little lime, magnesia or yttria (yttrium oxide, Rare Earths, Cerium and Phosphors) into the crystals holds them in their high-temperature form. With enough (fully stabilised) the problem vanishes. With a little less (partly stabilised), small grains still try to change form when a crack reaches them; the swelling squeezes the crack shut, and the ceramic becomes remarkably tough. Hot stabilised zirconia also lets oxygen pass through it as charged atoms, the basis of the oxygen sensor.

What you need

Item For Notes
Heavy mineral sand Everything 50–500 kg of beach or river black sand
Panning dish, sluice or shaking table Concentrating Ore Dressing: Jigs, Tables and Flotation, Mining and Tunnelling
Strong electromagnet Removing ilmenite and monazite The Electromagnet
High-voltage source, 15–30 kV Electrostatic separator Static Electricity and the Leyden Jar, The Induction Coil
Ball mill: stoneware jar and flint pebbles Zircon flour Described in Portland Cement
Brick press, steel moulds Bricks, crucibles Screws, Nuts and Bolts, Hydraulic Presses and Rams
A kiln reaching 1,500–1,750 °C Firing Forced draught with preheated air, or electric (Electric Kilns and Furnaces)
Caustic soda, hydrochloric acid, iron pots Zirconia Lye and Potash, Hydrochloric Acid
Lime, magnesia Stabilisers Burnt limestone (Lime); burnt magnesite (Firebrick and Refractories)

Where to find it

Zircon occurs as small grains in granite and gneiss everywhere, and as tiny crystals in most sands. Because it is hard and heavy and does not rot, waves and rivers sort it into the black sand layers of beaches and river bars, together with black magnetite and ilmenite, red-brown rutile, garnet and honey-yellow monazite (Titanium, Rare Earths, Cerium and Phosphors). Look for dark streaks on beaches below granite country, especially after storms. Rich deposits line the coasts of eastern and western Australia, South Africa, Mozambique, Kerala in India, Sri Lanka, Florida and Brazil. A black sand that is 2–10 % zircon is worth working.

Recognising it: under a hand lens, zircon grains are glassy, clear, pale yellow, pink, brown or colourless, often stubby four-sided prisms with pointed ends. They scratch quartz, sink fast in water, do not stick to a magnet, and do not dissolve in boiling acid. Some glow yellow-orange under ultraviolet light (Arc Lamps, Neon and Fluorescent Lights).

Baddeleyite, natural zirconia, is rare: brown-black heavy grains and crystals in a few alkaline rocks and in some phosphate and copper ores (Phalaborwa in South Africa; Poços de Caldas in Brazil). If you find it, it saves the chemistry below.

Concentrating zircon sand

1. Wash heavy grains stay behind the bars; quartz runs off 2. Weak magnet lifts black magnetite 3. Strong electromagnet lifts ilmenite, then (closer) monazite; zircon and rutile stay 4. Electrostatic separator hot, dry sand, one grain thick electrode wire 15–30 kV earthed roll, heated 15–25 cm across brush zircon clings rutile flies off
Fig. 1 Separating zircon from black sand. Washing on a sluice or table removes the light quartz. A weak magnet then lifts magnetite, and a strong electromagnet lifts ilmenite and monazite. On the electrostatic separator, grains that conduct (rutile and any ilmenite left) lose their charge on the earthed roll and fly off; zircon clings and falls on the far side.
  1. Wash. Run the sand over a sluice or shaking table, or pan it (Ore Dressing: Jigs, Tables and Flotation). Quartz and shell wash away; the heavy minerals stay. Repeat until the sand is dark and heavy: a handful should feel like lead shot.
  2. Dry it on a hot iron plate.
  3. Magnet. Pass a lodestone or weak magnet over a thin layer to lift magnetite. Then feed the sand slowly past the poles of a strong The Electromagnet, close up: ilmenite comes off first, then, held closer and stronger, monazite, which you keep apart (it is mildly radioactive and holds the rare earths).
  4. Electrostatic separation. What is left is mostly zircon and rutile. Rutile conducts electricity a little; zircon does not.

The electrostatic separator

An electrostatic separator sorts dry grains by whether they conduct electricity.

  • The roll: an earthed iron or brass drum 15–25 cm across and 30–60 cm long, turning at 100–300 turns a minute, heated to 80–150 °C (warm grains conduct better and carry no damp).
  • The electrode: a thin wire or a fine-toothed bar, parallel to the roll, 3–6 cm from it, charged to 15–30 kilovolts by a static machine or an induction coil with a rectifier (Static Electricity and the Leyden Jar, The Induction Coil, Rectifiers: Turning AC into DC). It sprays charge onto every grain passing under it.
  • The feed: a hopper with a vibrating tray that spreads dry, hot sand one grain thick onto the top of the roll.

Grains that conduct (rutile, ilmenite) hand their charge to the earthed roll at once and are thrown off by the spin. Grains that do not conduct (zircon, monazite, garnet, quartz) keep their charge, cling to the roll, and are brushed off underneath into a separate bin. Pass the zircon fraction two or three times. Good zircon concentrate is pale cream to buff, glistening, and 95 % or more zircon grains when you count them under a lens.

Zircon flour

Most uses need zircon ground fine. Grind it wet in a ball mill (Portland Cement): a stoneware jar a third full of zircon sand, a third full of hard flint pebbles, topped with water, rolled at about two-thirds of the speed at which the pebbles would stick to the wall and turn with it. Zircon is harder than flint and wears the pebbles; grinding to under 10 thousandths of a millimetre takes 2–4 days. Settle, pour off the water, and dry. Rub a pinch between your teeth: good opacifier flour feels like flour, with no grit.

Zircon mould wash and foundry sand

Zircon makes the face of a mould that steel cannot burn into (Metal Casting):

  • Facing sand: zircon sand mixed with 3–5 % plastic clay and enough water to hold together when squeezed, rammed 2–3 cm thick against the pattern, and backed with ordinary moulding sand. It conducts heat away fast (chilling the casting's skin), hardly expands, and does not react with molten iron oxide, so castings come out clean.
  • Zircon mould wash is a paint for mould and core surfaces: 100 parts zircon flour, 4–5 parts plastic clay, 1–2 parts dextrin (Glues and Adhesives), and water to the thickness of cream. Brush or spray it 0.3–0.5 mm thick and dry the mould thoroughly, or mix it with alcohol and burn the alcohol off with a match. Good wash covers evenly, does not crack or flake when dry, and does not rub off on a finger.

Zircon bricks

A zircon brick is a dense refractory brick made almost entirely of zircon. Use it where molten glass, aluminium or acid slag touches the lining: the throat and walls of a glass tank (Glass), the floor of an aluminium melting furnace (Aluminium), pouring nozzles for steel (Steel in Quantity).

  1. Mix, by weight: 55 zircon sand as it comes from the separator, 40 zircon flour, 5 plastic clay or kaolin as a binder, and 3–5 % water. The coarse grains form the skeleton; the flour packs the gaps.
  2. Press the damp mix into a strong steel mould the size of your firebricks (Firebrick and Refractories), as hard as your press allows: a screw or hydraulic press (Hydraulic Presses and Rams) giving 300 atmospheres or more. Hand-rammed bricks work but are more porous.
  3. Dry slowly for a week.
  4. Fire to 1,500–1,600 °C and hold for 4–6 hours. This needs a forced-draught kiln with preheated air, or an electric kiln with silicon carbide elements (Electric Kilns and Furnaces). With 5 % feldspar added, bricks sinter at 1,400–1,450 °C, but stand less heat.

Good from bad. A zircon brick is far heavier than a firebrick of the same size: about 3.6–3.9 kg per litre of brick, against 2.0–2.3 for fireclay. It rings when tapped, has sharp edges, and drinks only a little water (weigh it dry and after an hour's boiling: under 5 % gain; ordinary firebrick takes up 8–15 %). A brick that crumbles at the edges or drinks a lot was underfired or under-pressed.

Glaze opacifier

Clear glaze light reaches the body: you see the dark stripe With 10–12 % zircon flour grains scatter light back: the glaze looks white glaze clay body dark stripe zircon grains
Fig. 2 How a zircon opacifier works. In a clear glaze, light passes through the glass and shows the clay body beneath. With 10–12 % fine zircon flour, the tiny zircon grains, which bend light much more strongly than glass, scatter it back out, so the glaze looks white and hides the body.

A glaze opacifier is a fine powder that turns a clear glaze white and hides the clay beneath it. Zircon flour is the cheapest and best in most glazes, and leaves tin oxide for where nothing else will do.

  1. Grind zircon flour as fine as you can: the finer, the whiter, for less.
  2. Test. Add 0, 4, 8, 12 and 16 % zircon flour to five batches of your clear glaze (Glazes), and paint them over a dark clay tile with a black stripe. Fire. Choose the lowest amount that hides the stripe; usually 8–12 % at earthenware heat and 10–15 % at stoneware heat. Tin oxide needs only 5–10 %, but costs far more.
  3. Adjust. Zircon stiffens a glaze. If the glaze turns dry, matt or pinholed, add a little more flux (Glazes).

It works in glazes from about 1,000 °C to 1,300 °C and in white enamels for iron (Enamel on Metal). Some zircon dissolves at top heat and grows back as tiny new crystals while cooling, which adds to the whiteness. Fired with a trace of vanadium, praseodymium or iron and a little fluoride flux at about 1,000 °C, zircon also makes stable blue, yellow and coral-pink colours for glazes, the zircon stains.

Making zirconia

Zircon flour + caustic soda Fuse 600–650 °C, 1–2 h Leach in water silicate dissolves Dissolve in acid hydrochloric Crystallise oxychloride needles Calcine 900–1,000 °C liquid kept: water glass iron and titanium stay in the liquid white zirconia powder
Fig. 3 From zircon to zirconia. Fusing with caustic soda breaks zircon into a sodium zirconate and a soluble silicate; water washes the silicate out; acid dissolves the zirconium, which crystallises clean as oxychloride; heating the crystals leaves pure zirconia.

Zircon holds its zirconium locked to silica. Break the lock with alkali:

  1. Fuse. In an iron pot, melt 1.2 kg caustic soda (Lye and Potash) and stir in 1 kg zircon flour a little at a time. Hold at a dull red heat, 600–650 °C, for 1–2 hours, stirring with an iron rod. The zircon becomes sodium zirconate and sodium silicate.
  2. Leach. Cool, break up the cake, and boil it in water several times. The sodium silicate dissolves; keep the liquid, it is Water Glass (Sodium Silicate). A white, sandy residue stays behind.
  3. Dissolve the residue in warm hydrochloric acid (Hydrochloric Acid), about 1 litre of strong acid per kilogram. Filter off any unreacted zircon.
  4. Crystallise. Boil the solution down and cool it. White needles of zirconium oxychloride grow. They are much less soluble in strong acid than iron and titanium salts, so dissolving them in fresh strong acid and crystallising again leaves almost all impurities behind.
  5. Calcine the crystals in a fireclay dish, outdoors, at 900–1,000 °C for 2 hours. They give off choking acid fumes and leave zirconia, a fine white powder. Expect about 0.5 kg from each kilogram of zircon.

Industry also melts zircon with coke in an The Electric Arc Furnace: the silica boils away and fused zirconia remains. Zirconia from any route carries about 2 % of a twin element, hafnium. For ceramics that does not matter.

Zirconia crucibles

A zirconia crucible holds metals and glasses up to about 2,000 °C: platinum (Platinum and the Platinum Metals), special steels and nickel alloys (Alloy and Stainless Steels), and optical glass that must not pick up clay (Optical Glass and Achromatic Lenses).

  1. Stabilise. Mix zirconia powder with 5–7 % by weight of lime (from burnt limestone, Lime) or 3–4 % magnesia (from burnt magnesite). Moisten, press into cakes, and fire as hot as you can, 1,600 °C or more, for several hours so the lime dissolves into the zirconia.
  2. Grade the grain. Crush the fired cakes. Mix 60 parts grains of 0.1–1 mm with 40 parts fine powder. Graded grain resists cracking from sudden heat.
  3. Shape. Moisten with 3–4 % of dextrin solution and ram it hard into a steel or graphite mould around a tapered core: walls 5–8 mm for a 100 ml crucible, a rounded inside base. Or slip-cast fine stabilised powder in plaster (Slip Casting, Jiggering and Ceramic Factories).
  4. Dry a week; fire to 1,650–1,750 °C, rising slowly through 1,000–1,300 °C. A carbon-arc or induction furnace with a graphite tube around the work reaches this (Electric Kilns and Furnaces).

Good from bad. A good crucible is cream to ivory, dense, rings clearly, and survives five cycles of being heated to 1,200 °C and cooled without cracking or crumbling. If it crumbles to powder after a few heatings, it was not stabilised: more lime, higher stabilising fire. Its weakness is sudden heat: always warm it slowly. For melting glass or aluminium at up to 1,600 °C, a zircon crucible (zircon flour with 5–10 % kaolin, fired at 1,500 °C) is easier to make and good enough.

Zirconium metal, in outline

Zirconium metal looks like steel, weighs less, and shrugs off boiling acids and alkalis. It cannot be smelted with carbon. The route, a large undertaking for a later age:

  1. Chlorinate: heat zircon with carbon in a stream of chlorine at 800–1,200 °C. Zirconium chloride comes off as a vapour and condenses as a white solid at about 330 °C; silicon chloride stays a gas until much colder.
  2. Reduce (the Kroll process): drip the purified chloride vapour onto molten magnesium (Magnesium) at about 850 °C in a sealed steel pot filled with argon (Liquid Air, Nitrogen and the Noble Gases). The result is a porous sponge of zirconium in magnesium chloride.
  3. Clean the sponge by boiling off the magnesium and its salt in vacuum (The Vacuum Pump), then melt it in a vacuum arc furnace.

For nuclear fuel tubes the hafnium must first be removed, because it soaks up neutrons; that needs a long chemical separation.

How to tell it worked

  • Zircon concentrate: pale, glistening, heavy; a pinch on white paper shows no black grains; a magnet lifts nothing.
  • Opacified glaze: white, smooth and glossy, hiding a black stripe beneath.
  • Bricks and crucibles: heavy, ringing, no cracks after a full firing and cooling.

Note Troubleshooting.

  • Zircon still dark after separation → ilmenite left; slower feed, stronger magnet, hotter roll.
  • Electrostatic separator sorts nothing → sand damp or cold, or the electrode too far from the roll.
  • Glaze speckled, not white → flour too coarse; grind longer.
  • Zirconia crucible cracks on first cooling → not stabilised; cracks on heating → heated too fast, or grain not graded.
  • Fused cake will not leach → too little caustic or too cool; grind and fuse again.

Dangers

Danger Caustic, acid and fumes. Molten caustic soda destroys skin and eyes instantly; a drop of water into it explodes it out of the pot. Wear a face shield, leather gloves and apron; add zircon slowly and dry. Calcining oxychloride and the chlorine of the Kroll route give off poisonous gases: work outdoors, upwind, and never alone (Chlorine and Bleach).

Danger Burning metal. Zirconium powder, fine turnings and sponge can catch fire by themselves in air and burn white-hot. Water and wet sand make it worse. Smother with dry sand, and keep fine scrap under water or oil until it is melted.

What this unlocks

Better glass tanks and cleaner Glass; clean steel castings (Metal Casting); cheap white sanitaryware, tiles and enamel (Slip Casting, Jiggering and Ceramic Factories, Laying Tiles and Mosaics, Enamel on Metal); crucibles for platinum and superalloys (Alloy and Stainless Steels); piezoelectric ceramics (Piezoelectric Crystals and Ceramics); thermal barrier coatings (Jet Engines); oxygen sensors for engines (The Internal Combustion Engine); cubic zirconia (Synthetic Gems); and fuel cladding for Nuclear Energy (Overview).

How it was first done

Zircon has been cut as a gem since antiquity, called hyacinth or jargoon, much of it from Sri Lanka. In 1789 the German chemist Martin Heinrich Klaproth found a new earth, zirconia, in zircon from Ceylon, and in 1824 Jöns Jacob Berzelius made the first impure zirconium metal. Anton Eduard van Arkel and Jan Hendrik de Boer at Philips in Eindhoven made the pure, ductile metal in 1925 by splitting its iodide vapour on a hot wire. Zircon opacifiers began replacing costly tin oxide in glazes and enamels in the 1920s and 1930s. In the 1940s William Kroll, working with the United States Bureau of Mines, adapted his magnesium process to zirconium, and from the 1950s zirconium alloy tubes carried the fuel of naval and power reactors. In 1975 Australian researchers led by Ron Garvie showed that partly stabilised zirconia could be as tough as some metals, calling it "ceramic steel", and in the early 1970s Soviet scientists at the Lebedev Institute grew large cubic zirconia crystals by melting the powder inside a shell of its own unmelted powder.

Source: content/entries/earth/zirconium.md