◆ Rebuild

Part 3 · Metals

Files and Saws

A file is a bar of hardened steel covered in tiny chisel teeth, cut one blow at a time; a saw is a thin steel strip with a row of bent teeth. With files you can shape any metal part by hand; with saws you can turn logs into boards. Both are made from steel with nothing but a chisel, a hammer and patience.

Difficulty
●●●●●
Time
A day to cut and harden a small file; two days to make a frame saw blade; an hour to sharpen a saw
Steps from zero
13 prerequisites →

You need first

Steel

This unlocks

Sawmills and LumberPlanes, Drawknives and Woodworkers' Tools

Objects made here

filebow sawpit sawraspsaw
The full path from nothing — 13 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel
  14. Files and Saws

Do them roughly in this order. See it on the tech tree →

Why it matters

Once metal is forged, it is still rough. To make a lock, a hinge that closes cleanly, a screw thread, a gear tooth, a bearing or a valve, you must remove metal precisely — a tenth of a millimetre at a time. Before machine tools, that meant the file. Clockmakers, gunsmiths, locksmiths and instrument makers built everything from the The Mechanical Clock to the first The Steam Engine valve gear largely with files. Files also sharpen saws and shape the teeth of Gears; rasps shape wood, horn and hooves.

The saw turns trees into boards. With only axes, a whole log yields one or two thick planks, hewn and split. With a saw, the same log gives a dozen thin, straight boards — enough for floors, doors, Furniture, boats, barrels, boxes and the frames of machines. A saw powered by a The Waterwheel became the first sawmill.

Both are steel tools with many small teeth, so they are made with the same skills, and you need a file to sharpen a saw. Rigid handsaws, hacksaws and the rest of the carpenter's saws are in Planes, Drawknives and Woodworkers' Tools.

How it works

A file is a row of tiny chisels. Each tooth is a ridge raised by a chisel blow, with a steep face toward the point of the file. Pushed across softer metal, each ridge shaves off a tiny chip. Because the file is hardened to glass-hardness, it cuts anything softer than itself: iron, unhardened steel, bronze, brass, copper, wood, bone and horn.

You do not need a file to make a file. The blank is ground flat on sandstone while it is soft, the teeth are raised with a hardened chisel, and only then is it hardened. Almost every file in the world before the mid-1800s was cut this way, by hand, a blow at a time.

A saw is a row of tiny chisels or knives on a thin plate, with spaces (gullets) between them to carry the sawdust out. If the teeth were straight, the plate would jam in its own cut. So alternate teeth are bent slightly to each side: this is the set. It makes the cut (the kerf) wider than the plate, so the saw runs freely.

Wood is cut in two ways, and the teeth differ:

  • Ripping — cutting along the grain, to make planks. The teeth are little chisels that chop the fibres off at the bottom of the cut.
  • Crosscutting — cutting across the grain, to cut boards and logs to length. The teeth are little knives with pointed, bevelled tips that sever the fibres on each side of the cut before they are torn out.

What you need

Item Notes
High-carbon steel For files, the hardest steel you have (about 1% carbon or more); for saws, 0.6–0.8%. See Steel.
Forge, anvil, hammers, tongs See Blacksmithing
Grindstone and flat sandstone slabs To grind blanks flat. See Axes, Chisels, Knives and Planes.
File-cutting chisels Short, hardened steel chisels, a little wider than the file, edge about 50°
File-cutting hammer 0.5–1 kg, with a face you can see past
A lead or tin bed A slab 1 cm thick on the anvil, to support the teeth already cut. See Lead or Tin and Pewter.
Leather strap Loop passed over the blank and held down by your feet
Hardening paste Fine charcoal or charred bone, horn or leather powder, Salt, a little flour and water
Brine quench One cupful of salt per 4 L of water, 20 L or more
For saws Thin steel strip, a triangular file, a flat file, a notched setting bar or a small punch, two clamping boards
Saw frames Straight-grained ash, beech or hornbeam; strong cord (see Cordage and Rope)

Where to find it

The steel comes from Steel, carburised and folded until even. Lead for the cutting bed is smelted from galena (see Lead); a bed of tin, pewter or even a smooth slab of very hard, close-grained wood (end grain up) will do for a first file, though the teeth on the first side get slightly flattened. Frame wood is straight-grained ash, beech, hornbeam or hickory, split and seasoned (see Basic Woodworking).

Method 1: Cutting a file

You sit here 12° strike, repeat slide to the ridge, Chisel top leans toward you Teeth face the point Tang away from you Lead bed cushions the teeth underneath Anvil Tooth patterns, seen from above Single cutone course at 65–70° Double cut45°, then 70–80° across Raspteeth punched one by one coarse 8–10 teeth per cm · smooth 16–24
Fig. 1 Cutting a file by hand. The chisel leans toward you; each blow raises a ridge just beyond it, and the chisel is slid forward until it stops against that ridge. Below, the three common tooth patterns.

Make the blank

  1. Forge a bar of high-carbon steel into the file shape. A good first file is a flat bastard file: 20–25 cm long, 20–25 mm wide, 5–6 mm thick, tapering slightly in width and thickness over the last third toward the point. Draw out a square tang 6–8 cm long at the other end for the handle.
  2. Anneal it: heat it to an even cherry red and bury it in a bucket of hot wood ash or charcoal dust to cool as slowly as possible, overnight. It must be dead soft for cutting.
  3. Grind it flat. Rub the faces on a flat sandstone slab with water, or on the grindstone, until they are flat and smooth, with no hammer marks and no scale. Any pit left now will be a bald spot without teeth.

Cut the teeth

  1. Set up. Put the lead slab on the anvil. Lay the blank on it with the tang pointing away from you. Pass a leather strap over each end of the blank and down to loops under your feet, so your feet hold the blank tight.
  2. Hold the chisel across the file at the angle you want the teeth (see below), with its edge on the blank at the point end nearest you. Lean the top of the chisel toward you, about 12° from upright.
  3. Strike once, firmly. The chisel sinks in and throws up a small sharp ridge just beyond it, on the side away from you.
  4. Slide the chisel forward, keeping it on the blank, until you feel it stop against the ridge you just raised. Strike again. The ridge itself spaces the next tooth — you never measure.
  5. Keep the rhythm: slide, strike, slide, strike, all the way to the tang end. Every blow must be the same weight. A heavier blow raises a bigger ridge and wider spacing; a lighter one, finer teeth.

Angle and pattern:

Pattern How For
Single cut One course of parallel teeth at about 65–70° to the length of the file Sharpening saws and edge tools; a smooth finish
Double cut A first course at about 45° (the overcut), then a second, slightly lighter course across it at about 70–80° the other way (the upcut) General metal removal; fastest cutting
Rasp Separate pointed teeth raised one by one with a narrow pointed punch, in staggered rows Wood, horn, hoof, leather

Grade comes from the spacing. Roughly: coarse (bastard) 8–10 teeth per cm; second cut 12–14 per cm; smooth 16–24 per cm. Your first files will be coarse.

  1. The other face. Turn the file over onto the lead bed. The soft lead takes the shape of the teeth on the underside and stops them being crushed. Cut the second face the same way.
  2. Edges. Cut one edge with a single course; leave the other uncut as a safe edge, so you can file into a corner without cutting the side wall.
  3. Check the feel. Rub your thumb lightly from the point toward the tang: it should catch on every tooth. From tang toward point, it should slide. If it is the other way round, the teeth face backward — your chisel was leaning the wrong way.

Other shapes. Half-round and round (rat-tail) files are forged in grooved swages and cut on a lead bed with a matching groove, turning the file a little after each row. Three-square (triangular) files, the ones used for saws, are forged triangular and cut on each of the three faces in a V-groove in the lead.

Harden the file

  1. Coat it. Mix fine charcoal powder (better: charred horn, hoof or leather) with salt, a little flour and water into a thin cream. Paint it over the teeth and let it dry. It stops the teeth from scaling and from losing carbon at the surface — a file whose teeth lose their carbon is useless.
  2. Heat evenly in a clean, deep charcoal fire, away from the direct blast, to an even cherry red — just past where a lodestone stops sticking (see Steel). The thin point heats fastest; keep it toward the cooler side.
  3. Quench straight down, point first, into brine, moving it up and down — never sideways — until the hissing stops.
  4. Soften the tang. A glass-hard tang snaps off. Hold the tang (only) against a red-hot bar or in red-hot tongs until it turns blue, then let it cool.
  5. Temper lightly or not at all. Files are left nearly fully hard. Warming the body in boiling water for 15 minutes relieves strain and reduces cracking without softening the teeth.
  6. Clean with a stiff brush and water, dry it at once, and oil it.

Method 2: Making a saw

The easiest saw to make is the frame saw (bow saw): a thin, narrow blade held tight in a wooden frame. Because the frame keeps it in tension, the blade does not need to be stiff, perfectly flat or even fully hardened — which makes it far easier to forge than a free-standing handsaw.

The blade

  1. Forge a strip of steel 50–80 cm long, 2.5–4 cm wide and about 0.8–1 mm thick. This is slow: work it in short sections, at an orange heat, on a clean, flat anvil face, overlapping your blows. (See Sheet Metal and Rolling for hammering thin strip in packs and with water power.)
  2. Flatten and grind. Hammer out kinks cold on a flat anvil with light blows, then grind both faces smooth on sandstone.
  3. Drill or punch a hole 5–6 mm across at each end, 1 cm from the end, for the pins that hold it in the frame.
  4. Heat treat. Harden the whole strip in warm oil or melted fat (water warps and cracks thin strip), then temper it evenly to blue (about 300 °C) on a hot iron plate or in hot sand. It will be springy, but soft enough for a hard file to cut. A first blade can also be left unhardened and just cold-hammered stiff; it works, but needs sharpening far more often.

Laying out and cutting the teeth

Rip teeth along the grain: little chisels Crosscut teeth across the grain: little knives front face upright front leans back 10–15° cutting stroke cutting stroke seen from above: filed straight across (90°) seen from above: filed at 65–75°, alternating Set teeth seen end-on kerf ≈ 1½ × plate top half of each tooth bent, in turn left and right saw plate
Fig. 2 Saw teeth. Rip teeth are little chisels filed straight across; crosscut teeth are little knives filed at an angle. Setting bends alternate teeth outward so the cut is wider than the plate.
  1. Mark the spacing (the pitch). Clamp the blade between two boards with its edge just showing. Walk a pair of dividers along it, or copy the marks from a wooden strip marked out once with care.
Saw Pitch (tip to tip)
Fine crosscut, for joinery 2.5–3.5 mm
General rip saw 4–6 mm
Frame saw for green logs 5–8 mm, deep gullets
Pit saw 15–25 mm
  1. File the gullets with a triangular file, one stroke pattern per tooth, the same number of strokes and the same pressure each time, until every tooth comes to a point. Teeth are easiest to keep even if you file every second gullet along the blade, then turn the blade round and do the others.
  2. Shape:
    • Rip teeth: the front face is upright (at 90° to the line of the teeth), the back slopes at 60° — the shape a triangular file gives naturally. File straight across, at 90° to the blade.
    • Crosscut teeth: lean the front face back 10–15°, and hold the file at 65–75° to the blade (not square), alternating the angle from tooth to tooth. Each tooth gets a bevelled, knife-like point on its outer side.
  3. Set the teeth. Bend the top half of every second tooth one way, then turn the blade over and bend the others the other way. Either use a wrest — a hardened bar with notches — to twist each tooth gently, or lay the blade on a hardwood block with a slightly bevelled edge and tap each tooth over the bevel with a small punch. Aim for a kerf about 1½ times the thickness of the plate: more for soft green wood, less for dry hardwood. Every tooth must be set equally, or the saw will wander toward the side with more set.
  4. Joint the teeth: run a flat file lightly along the tops, lengthways, until each point shows a tiny flat shiny spot. Now all teeth are the same height.
  5. Sharpen: file each tooth again, just until its shiny spot disappears. Stop there.

The frame

Frame saw (bow saw) Toggle twist to tighten doubled cord Stretcher Blade 0.8–1 mm, held taut arm and handle; pin through blade Pit saw Top sawyer guides, lifts Squared log chalk line top and bottom cross-beam cuts on the downstroke Pitman pulls down; broad hat pit about 1.8 m deep, 1 m wide
Fig. 3 A frame saw (left) and a pit saw (right). The frame saw's blade is held tight by twisting the cord with a toggle. In the pit saw, the top sawyer guides and lifts; the pitman below pulls the cutting stroke.
  1. Make two arms of ash or beech, 45–60 cm long, 3 × 2 cm, and a stretcher a little longer than the blade, with tenons at each end that sit loosely in mortises at the middle of the arms.
  2. Saw a slot in the lower end of each arm for the blade; drive an iron pin through arm and blade hole.
  3. Tie a doubled cord between the upper ends of the arms. Put a flat stick (the toggle) between the strands and twist. As the cord shortens, it spreads the lower ends and pulls the blade tight. Lock the toggle against the stretcher.
  4. Twist until the blade rings with a clear note when plucked and does not flex sideways under your thumb. Slacken it after use so the frame does not take a permanent set.

The pit saw

To make planks from big logs, two people work a long saw up and down through a log laid over a pit.

  • The saw: an open blade 1.6–2.4 m long, about 2 mm thick, 15–20 cm wide at the top tapering to 8–10 cm at the bottom, with a crosswise wooden handle at each end; or a thinner blade stretched in a rectangular wooden frame. Teeth 15–25 mm apart, all raked to cut on the downstroke only.
  • The pit: about 1.8 m deep, 1 m wide and longer than the logs, with two strong cross-beams over it. On wet ground, build a high trestle instead.
  • Preparing the log: hew it square with an axe (see Axes, Chisels, Knives and Planes). Snap a cord rubbed with charcoal or chalk along the top and the bottom to mark each cut.
  • Sawing: the top sawyer stands on the log, guides the saw along the line and lifts it. The pitman below pulls the cutting stroke and wears a broad hat against the sawdust. Drive wedges into the kerf behind the saw so the cut does not close on it.

How to tell it worked

  • A good file bites at once into soft iron, leaving bright, even scratches, and does not skate. Another hardened file skates across it without biting. Its teeth stay sharp after a day's work on iron.
  • A good saw starts a cut easily, runs straight along a line without being forced, and leaves a kerf of even width. Sawdust from ripping is coarse and chippy; from crosscutting, finer.
  • Even teeth: sight along the jointed teeth — every point should line up. Look down the blade from the end: the set teeth should form two even rows.

Note Troubleshooting. File skates over iron → not hard (not enough carbon, too cool, quenched too slowly), or the teeth lost their carbon in the fire. Use the hardening paste, a hotter and more even heat, and brine. File teeth crumble → overheated before quenching. Keep it to cherry red. File cuts on the pull stroke instead of the push → teeth face backward. Lean the chisel the other way. Uneven, bald patches on the file → blank not ground flat, or blows uneven. Grind flatter and practise rhythm on scrap. Saw wanders to one side → more set on that side, or teeth sharper on one side. Joint, re-set evenly, and sharpen. Saw binds and jams → too little set, or the wood is closing on it. Add set; wedge the kerf. Teeth break off when setting → blade too hard. Re-temper to full blue or slightly beyond.

Dangers

Danger File tangs. A file used without a handle can drive its pointed tang deep into your palm or wrist. Always fit a wooden handle with an iron or copper ferrule before using a file, even for a moment.

  • Flying chips. Hardened files snap like glass and can throw sharp pieces. Never hammer on a file or use it as a pry bar.
  • Lead. Do not eat or drink while working on a lead bed, and wash your hands afterward. See Lead.
  • Saw cuts. Saw teeth cut deep, ragged wounds. Carry saws with a slotted wooden guard over the teeth.
  • Pit sawing. A log can roll off the cross-beams onto the pitman. Wedge and chock it firmly before sawing. The pitman should wear a hat and cover his eyes from the sawdust.

What this unlocks

With files you can fit metal parts: Locks and Keys, Screws, Nuts and Bolts, Gears, Springs, the parts of the The Mechanical Clock and the The Steam Engine. With saws you get planks for Furniture, Barrels and Cooperage, Boats and Sails, Timber Framing and Log Building and Roofs. Harnessing a frame saw to a The Waterwheel with a crank (see Cranks, Cams and Linkages) gives a sawmill. In time, files are replaced for heavy work by Machine Tools — but even then, the final fitting is done by hand with a file.

How it was first done

Egyptian carpenters used copper and bronze saws by about 3,000 BC, mostly pulled rather than pushed; copper saws were also used with sand to cut stone. Rasps of bronze are known from ancient Egypt, and iron files from the Assyrian empire by the 7th century BC. Roman woodworkers had frame saws, pit saws and saws with teeth set alternately to each side — the Roman writer Pliny the Elder describes setting the teeth to clear the sawdust. A Roman water-powered stone saw driven by a crank and connecting rod is carved on a tomb at Hierapolis, in modern Turkey, from the 3rd century AD. The Viking tool chest found at Mästermyr in Gotland (about AD 1000) contained several files. Files were cut entirely by hand, in the way described here, until file-cutting machines spread in the mid-1800s; hand file-cutters in Sheffield, England, worked this way into the 20th century.

Source: content/entries/metals/files-and-saws.md