◆ Rebuild

Part 7 · Home and Daily Life

Linoleum, Oilcloth and Floorcloths

Linseed oil hardens in air into a tough, waterproof skin. Painted onto canvas it makes floorcloths, wipe-clean oilcloth table covers, tarpaulins and painted canvas; oxidised, mixed with resin and cork or wood flour and pressed onto jute, it makes linoleum — a warm, hard-wearing, washable floor.

Difficulty
●●●●●
Time
A few weeks for a floorcloth or oilcloth (mostly drying time); two to three months for linoleum by the old method
Steps from zero
8 prerequisites →

You need first

Oils and PressingThe Loom

This unlocks

—
The full path from nothing — 8 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Simple Machines
  4. Basic Woodworking
  5. Farming from Seed
  6. Spinning and Weaving Cloth
  7. Oils and Pressing
  8. The Loom
  9. Linoleum, Oilcloth and Floorcloths

Do them roughly in this order. See it on the tech tree →

Why it matters

A bare earth or board floor is cold, dusty and hard to clean. A floorcloth — heavy canvas painted thick with oil paint — gives a smooth, warm, washable floor that lasts for years, and can be made by one person with a brush. Oilcloth does the same for tables, shelves and children's bibs: food and spills wipe off. Tarpaulins keep rain off haystacks, wagons, boats, woodpiles and tents. Linoleum, the industrial version, was the standard floor of kitchens, hospitals, schools and ships for a century: it is hard-wearing, quiet underfoot, easy to keep clean and made entirely from plants and chalk.

All of these rest on one material: linseed oil from the seed of flax (Oils and Pressing), and one skill: weaving strong cloth (The Loom, Ropewalks and Sailcloth).

How it works

Drying oils. Linseed oil does not dry by evaporating like water. It takes oxygen from the air, and its molecules link together into a tough, rubbery solid, the way milk sets into cheese. A thin film gains weight as it dries (it is taking in oxygen) and becomes a skin that water cannot pass. This is why oil paint, varnish and putty work (Pigments, Paints and Varnish).

Three things control it:

  • Thickness. Oxygen must reach the oil. A film thinner than a sheet of paper dries in days; a thick puddle skins over on top and stays liquid underneath for months, and then wrinkles. So every coating here is built up in many thin coats.
  • Warmth and light. Drying goes much faster warm and in daylight. A coat that dries in two days at 25 °C may take a week in a cold barn.
  • Driers. Small amounts of manganese (from the brown earth pigment raw umber, or from manganese ore) speed up the reaction many times. Oil heated with a drier is boiled oil: it dries in a day instead of a week.

Linoleum takes the same reaction much further. The oil is oxidised in bulk until it becomes a solid, elastic, cork-like material (old makers called it linoxyn). Cooked with resin it becomes a sticky dough called linoleum cement. Filled with cork or wood flour and chalk, pressed onto jute cloth and baked slowly, it sets into a sheet that is hard yet flexible, and keeps hardening for years.

What you need

Item Amount For See
Linseed oil 1 litre per 2–3 m² of floorcloth; much more for linoleum Everything Oils and Pressing
Raw umber or powdered manganese ore 1–2 % of the oil's weight Drier Pigments, Paints and Varnish
Heavy canvas (linen, hemp or cotton duck), 400–600 g/m² As needed Floorcloth, tarpaulin Ropewalks and Sailcloth
Close-woven cotton or linen, about 200 g/m² As needed Oilcloth Spinning and Weaving Cloth
Jute hessian (burlap) As needed Linoleum backing The Loom
Chalk (whiting), ochre, charcoal black Several kg Filler and colour Pigments, Paints and Varnish
Hide glue A little Size Glues and Adhesives
Rosin (pine resin), cork or fine sawdust See below Linoleum Tar, Pitch and Glue
Pine tar, beeswax, tallow As needed Tarpaulins Tar, Pitch and Glue
Broad knife or wooden straight-edge, brushes, pumice — Spreading and smoothing Brooms, Brushes and Combs

Where to find it

  • Flax gives both the oil (its seed, linseed) and linen cloth; hemp gives the heaviest canvas (Flax, Hemp and Linen).
  • Jute is a tall, fast-growing plant of hot, wet river plains, above all the Ganges delta of Bengal. Its long, golden, glossy bast fibre makes coarse, cheap hessian and sacking. Where there is no jute, coarse hemp or flax tow cloth does the same job.
  • Cork comes from the bark of the cork oak of the western Mediterranean. Without it, use fine sawdust sieved to flour ("wood flour") from pale, non-resinous woods such as poplar, lime, birch or willow.
  • Chalk (whiting) is soft white limestone ground and washed (Pigments, Paints and Varnish). Raw umber is a dark brown earth found with ochres, rich in manganese; it is the safest drier.
  • Rosin is what is left when pine resin is heated to drive off the turpentine (Tar, Pitch and Glue).

Making boiled oil

Every product here uses it.

  1. Work outdoors, away from buildings, with a close-fitting lid and a bucket of sand beside you.
  2. Warm the oil in an iron or copper pot over a small fire and stir in 1–2 % of its weight of finely ground raw umber or manganese ore.
  3. Keep it hot and stir for 2–3 hours. It should stay just below smoking: a slice of bread dropped in browns in about 10 seconds (roughly 200 °C). If it smokes heavily or foams up, pull it off the fire.
  4. Let it cool and settle for a few days, then pour off the clear, darker oil.

Test it: brush a thin film on glass. Boiled oil is dry to the touch within a day in warm weather; raw oil takes three to seven days. Sun-thickened oil (Pigments, Paints and Varnish) is a slower, safer alternative.

Floorcloth

FLOORCLOTH about 2 mm thick (layers not to scale) Varnish 2–3 coats of oil varnish Painted design stencilled or freehand Ground 3–4 coats of oil, chalk and ochre Size thin hide glue Canvas heavy linen, hemp or cotton OILCLOTH about 0.8 mm thick (layers not to scale) Varnish thin, flexible Printed pattern woodblock Coats 2–3 thin: more oil, less chalk Cloth close-woven cotton or linen LINOLEUM about 3 mm thick (layers not to scale) Wax beeswax, polished Linoleum oxidised oil, resin, cork or wood Hessian jute, pressed into the mass Back coat paint or varnish
Fig. 1 The layers of a floorcloth, oilcloth and linoleum. Each is built from many thin layers; linoleum's body is a single thick layer of oxidised oil, resin and cork pressed into jute.
1. STRETCH AND SIZE 2. GROUND COATS 3. DESIGN AND VARNISH Canvas tacked to a frame or floor, 5 cm oversize; brush on thin glue size so oil cannot rot the fibres. Spread thick paint (boiled oil, chalk, ochre) with a broad knife. 3–4 coats, a week apart; rub each smooth with pumice when hard. thin, even coat Stenciloiled card or thin leather; dab colour with a stiff brush. Then 2–3 coats of varnish.
Fig. 2 Making a floorcloth: stretch and size the canvas, build up thin ground coats with a broad knife, then stencil the design and varnish.
  1. Canvas. Cut heavy canvas 5 cm larger all round than the finished size. If you must join widths, overlap them 3 cm and sew a flat double seam, then hammer it flat.
  2. Stretch. Tack it tight to a wooden frame, or to a clean floor or wall, with tacks every 8–10 cm, pulling it square.
  3. Size. Brush on a thin coat of warm hide glue (about 1 part glue to 15 parts water) and let it dry. Size fills the fibres so the oil sits on top; oil soaked straight into raw canvas rots and embrittles it within a few years.
  4. Ground coats. Mix a thick paint of boiled oil and chalk, coloured with ochre, about as stiff as soft butter. Spread it thinly with a broad knife or a straight-edged board, pulling it along so it fills the weave. Let it dry hard — 5–7 days — then rub down any lumps with pumice and water. Repeat for 3–4 coats, on the back too if you can (one coat is enough there).
  5. Design. Paint a background colour, then add borders and patterns with stencils cut in oiled card or thin leather, dabbing colour through with a stiff brush, or print them with carved wooden blocks. Checks, diamonds and imitation tiles are traditional.
  6. Varnish with 2–3 thin coats of oil varnish (Pigments, Paints and Varnish) or boiled oil, each dry before the next.
  7. Finish the edges. Take it off the frame, trim it square, and either turn a 2–3 cm hem under and glue it down with thick paint, or leave a clean painted edge. Let it cure for 2–4 weeks before walking on it.

Sizes and thickness. A finished floorcloth is about 2 mm thick and weighs about 1.5–2 kg/m². Floorcloths were made from hearth-rug size up to whole rooms.

Care. Wipe with a damp cloth; never soak it. Rewax or revarnish every year or two where feet wear it. Lay it on a smooth floor: grit underneath wears through from below. Roll it only painted side out, and never when cold, or the paint cracks.

Oilcloth

Oilcloth is a lighter, more flexible floorcloth for tables, shelves, aprons, bibs, bags and book covers.

  1. Stretch close-woven cotton or linen, about 200 g/m², on a frame and size it as for a floorcloth, with weaker glue.
  2. Apply 2–3 thin coats of boiled oil mixed with less chalk than for a floorcloth — about equal parts by volume — so it stays flexible. Scrape each coat smooth with the edge of a long straight-edge drawn across the cloth while wet. Dry each coat 2–4 days in a warm room.
  3. Add a top colour and print a pattern with woodblocks (Printing).
  4. Finish with one thin coat of pale varnish.

A good oilcloth folds without cracking, wipes clean, and does not feel tacky in warm weather. If it stays tacky, the oil was raw or the coat too thick; hang it in a warm, light place for another week.

Tarpaulin

A tarpaulin is a large sheet of canvas made waterproof, with strong edges and rings for ropes.

  1. Sew canvas widths together with flat double seams, overlapping 3–4 cm, sewn with waxed thread at about 3 stitches per cm (Ropewalks and Sailcloth). A useful size is 4 × 5 m for a haystack or wagon, or 2 × 3 m for a shelter roof.
  2. Edge it all round with a turned double hem 4 cm wide, or with a sewn-on bolt rope.
  3. Grommets (sewn rope rings or metal eyelets) every 50–60 cm along the edges and at each corner, with a patch of extra canvas behind each corner.
  4. Waterproof it in one of three ways:
    • Oil: 2–3 coats of boiled oil with lampblack or ochre stirred in. The pigment shields the oil and the cloth from sunlight and makes it last years longer. Dry each coat 3–5 days.
    • Tar (the original tar-paulin): pine tar warmed and thinned with about a quarter of its volume of linseed oil, brushed in hot. Black, sticky and very durable; best for covers that never touch clothes or food (Tar, Pitch and Glue).
    • Wax: rub a block of beeswax and tallow, about 3 : 1, hard into the canvas, then warm it in the sun or with a warm iron so it melts in. Waxed canvas stays supple and can be re-waxed in a few minutes.
  5. Fold it loosely for storage, dry, and redress the coating every year or two.

Test: sag the tarpaulin between four posts into a shallow dish and pour in a bucket of water. After a day there should be no drips underneath and no damp patches on the underside.

Painted canvas

Canvas painted on both sides, or laid into wet paint, has many hard uses:

  • Decks and roofs. On a boat deck or a cabin roof of tongue-and-groove boards, paint the boards thickly, lay canvas on the wet paint, tack it every 5 cm along the edges, then give it 3 coats of oil paint. It is watertight and non-slip with sand sprinkled in the last coat.
  • Buckets, covers and wagon tilts. Fire buckets of sewn canvas, painted inside and out, hold water for years.
  • Pictures and signs. An artist's canvas is stretched on a wooden frame with wedges in the corners for tightening, sized with weak hide glue, given two thin coats of a ground of chalk ground in linseed oil, sanded smooth, and then painted (Pigments, Paints and Varnish).

Linoleum

corkchalkpigment 1. Oxidise the oil boiled oil flooded over hanging cloths daily, in a warm shed 2. Cook the cement ground skins + rosin (4 : 1), stirred hot to a rubbery dough 3. Mix knead in cork or wood flour, chalk and colour jute hessian mix 4. Press between warm rollers onto the hessian, 2–4 mm 5. Stove hang in a warm room, 50–70 °C, 2–4 weeks, until firm and springy
Fig. 3 Making linoleum: oxidise the oil, cook it with rosin into cement, knead in cork or wood flour, chalk and colour, press it onto hessian between rollers, and stove it in a warm room until it sets.

Linoleum is a factory product, but it can be made in small sheets by hand. Expect several trial batches before you get one that sets firm without cracking.

  1. Oxidise the oil. The original way: hang sheets of thin cotton cloth from rails in a warm shed (about 30–40 °C) and pour boiled oil down them every day. Each day's film dries on the last. After 6–8 weeks each cloth carries a skin 1–1.5 cm thick, rubbery and yellow-brown. Cut down the skins and chop or grind them. A faster way: blow air from a Bellows through boiled oil heated to about 80–100 °C in a pot, through a pipe with small holes at the bottom, for many hours a day over several days, until the oil has thickened into a stiff, stringy jelly that no longer flows.
  2. Make the cement. Heat the oxidised oil with rosin, about 4 parts oil to 1 part rosin by weight, in a pot over a gentle fire, stirring, until it is an even, sticky, rubbery dough. Keep it below smoking.
  3. Mix. While the cement is warm, knead in, by weight, roughly:
Ingredient Share
Linoleum cement 40 %
Cork flour or fine wood flour, sieved 30–35 %
Chalk (whiting) 20 %
Pigment (ochre, umber, charcoal black) up to 5 %

Knead until the colour is completely even, with no streaks. More cork makes a softer, warmer floor; more wood flour and chalk a harder one.

  1. Press. Lay a sheet of jute hessian on a flat, smooth table. Put strips of wood 3 mm thick along both edges as guides. Spread the warm mix over the hessian and press it down with a heavy, warm iron or wooden roller running on the guides, pushing the mix into the weave. In a factory the mix is pressed onto the hessian between heated steel rollers (a calender) in one pass.
  2. Stove. Hang the sheets, or lay them flat on racks, in a warm room at about 50–70 °C (too hot to keep your hand against a wall for long) for 2–4 weeks, until a thumbnail pressed hard leaves only a slight mark that slowly fades. Thicker sheets take longer.
  3. Finish. Paint the back with oil paint to protect the jute. Wax the face with beeswax and polish.

Linoleum is 2–4 mm thick for homes, up to 6 mm for ships and hard-wearing public floors. New linoleum has a yellowish cast ("drying-room bloom") that fades after a few weeks in daylight.

Laying. The floor beneath must be dry, smooth and level; every bump will show and wear through. Unroll the sheets and let them lie flat in a warm room for two days to relax. Lay them with the edges butted tight, cut with a sharp knife against a straight-edge, and either stick them down with a paste of flour and a little rosin or leave them loose with a weighted border.

Inlaid linoleum is made by cutting shapes from sheets of different colours and fitting them together like a jigsaw on the hessian before pressing, so the pattern goes right through and never wears off.

How to tell it worked

  • Floorcloth: hard, smooth, no tackiness; a coin dragged firmly across it does not cut through to canvas; a cupful of water left on it for an hour leaves no mark.
  • Oilcloth: folds without cracking; wipes clean; not sticky on a hot day.
  • Tarpaulin: no drips after a day of standing water.
  • Linoleum: bends round a 10 cm pole without cracking; a thumbnail leaves only a fading mark; edges do not crumble when cut.

Note Troubleshooting. Paint wrinkles like the skin on hot milk → coat too thick; scrape off, apply thinner. Stays tacky for weeks → raw oil, too little drier, cold or dark room, or a non-drying oil such as olive or rapeseed; add drier, move to warmth and light. Paint cracks and flakes → too much chalk, too little oil, or rolled when cold; add more oil to the mix. Canvas rotten under the paint after a few years → no size; size next time. Linoleum crumbles → oil not oxidised enough, or too much filler; oxidise longer, use more cement. Linoleum stays soft → not stoved long or warm enough. Linoleum cracks when bent → over-stoved, too much chalk, or too thin.

Dangers

Danger Oily rags, skins and sawdust catch fire by themselves. Linseed oil gives off heat as it takes up oxygen. Rags, cloth offcuts, oxidised skins or oily sawdust in a heap can heat up and burst into flame hours later, with nobody near. Linoleum works and floorcloth workshops burned down this way. Spread oily rags flat outdoors to dry, or keep them under water in a closed pot, or burn them at once.

Danger Hot oil fires. Linseed oil heated for boiling oil or cooking linoleum cement can ignite and cannot be put out with water, which makes it explode in a fireball. Work outdoors, never fill the pot more than half full, keep a lid and sand at hand, and smother any flame with the lid.

  • Lead driers. Old recipes used litharge or red lead as driers and white lead in grounds. They are poisonous; use manganese (umber) and chalk instead.
  • Rosin and tar fumes irritate the lungs and eyes. Work in the open air.
  • Slipping. A newly waxed floorcloth or linoleum floor is slippery; buff off excess wax.

What this unlocks

The same chemistry gives oil paints and varnishes (Pigments, Paints and Varnish), printing ink (Printing), oilskins and waxed clothing (Raincoats, Oilskins, Umbrellas and Rubber Boots), tents and ground sheets (Tents, Sleeping Bags and Camping Gear) and putty for glazing (Window Glass). Rubberised cloth (Rubber) and later plastic floor coverings (Early Plastics) followed linoleum. Floors and their finishes are in Stairs, Floors and Interior Finishes.

How it was first done

Sailors tarred and oiled canvas long before anyone wrote it down; the word tarpaulin — a tarred pall, or covering — was in English use by the early 1600s. Painted floorcloths were made in England from the early 1700s and were common in American homes by the late 1700s; large ones were painted on huge frames in specialist works. In 1844 Elijah Galloway patented kamptulicon, a floor covering of rubber and cork. Frederick Walton, an English rubber manufacturer, noticed the rubbery skin that formed on a tin of linseed paint, and in 1860 patented a way of making it in bulk by flowing oil over hanging cloth. He named his floor covering linoleum, from the Latin linum (flax) and oleum (oil), patented it in 1863, and opened a factory at Staines, near London, in 1864. Faster methods of oxidising the oil by blowing air through it followed in the 1870s. Linoleum became the standard floor of kitchens, hospitals and warships until vinyl replaced it in the 1960s; it has since come back as a natural, long-lasting floor.