◆ Rebuild

Part 3 · Metals

Copper Smelting

The first metal. Hammer native copper cold, then learn to turn green malachite into metal with charcoal, a clay crucible and a bellows — and cast it into tools.

Difficulty
●●●●●
Time
An hour to hammer a bead; a full day per smelt, after a week of preparing ore, charcoal and crucibles
Steps from zero
11 prerequisites →

You need first

Finding and Identifying OresCharcoalBellowsPottery

This unlocks

The BatteryCopper WireRectifiers: Turning AC into DCPots, Pans and KettlesThe Steam EngineBronzeGold and SilverMetal CastingSoldering and BrazingZinc and Brass
The full path from nothing — 11 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Bellows
  12. Copper Smelting

Do them roughly in this order. See it on the tech tree →

Why it matters

Copper is the easiest useful metal to make. It melts at a temperature you can reach with charcoal and a pair of bellows; its best ores are bright green and easy to recognise; and it can be hammered, bent, drawn, cast and re-melted again and again without being lost. With copper you get awls that pierce leather, needles, fish hooks, chisels and knives that can be resharpened, and — mixed with a little tin — Bronze, the first metal hard enough to replace stone for good.

Copper also leads far beyond tools. It conducts electricity better than any common metal, which makes it the heart of Copper Wire, the The Battery, electromagnets and the The Generator. Mixed with zinc it becomes brass. Every one of those starts with the skills in this chapter.

How it works

Copper ore is copper joined to other things. Green malachite, for example, is copper locked up with carbon dioxide and water. Smelting takes three steps, which all happen inside a hot bed of charcoal:

  1. Heat breaks the ore. Above about 300 °C, malachite gives off its water and carbon dioxide and turns into black copper oxide.
  2. Carbon steals the oxygen. Charcoal burning with too little air makes carbon monoxide gas (CO). This gas grabs oxygen from the copper oxide and leaves metallic copper. This is called reduction. It starts at a dull red heat, but the copper is left as tiny specks unless the heat goes higher.
  3. Heat melts the copper out. At 1,085 °C — a bright orange to yellow heat — copper melts. Its droplets run together into beads called prills and sink, because copper is three times heavier than the rocky waste around it. The waste rock, if it gets hot enough, melts into a glassy slag that floats on top.

The two most important lessons follow from this. First, the fire must be hot and smothered at the same time: deep in charcoal, with air coming in, but with no free air reaching the copper — or it will burn back into oxide. Second, the cleaner your ore, the better: every bit of rock you pick out by hand is rock you do not have to melt.

What you need

Item Amount Notes
Copper ore — malachite or azurite 0.5–2 kg per smelt Hand-picked, crushed. See Finding and Identifying Ores. Native copper needs no smelting at all.
Charcoal 5–10 kg per smelt Pieces 1–3 cm, plus a bag of fine powder. See Charcoal.
Bellows One pair, or 3–4 blowpipes for a tiny crucible See Bellows.
Tuyere 2–3 Fired clay pipe, see Bellows.
Crucibles 3–4 Fired clay pots, see below.
Hammerstones and an anvil stone A smooth hard river cobble (1–2 kg) and a flat-topped boulder. See Stone Tools.
Green-wood tongs 2 A split green sapling, 60–80 cm, bound behind the split; or two green sticks lashed in an X.
Mould 1 Carved stone or fired clay, see below.
Water A bucket For quenching — never near the pour.

Making a crucible

A crucible is a small thick pot that holds metal in the fire. It must not crack or melt.

  1. Mix Finding and Preparing Clay with an equal volume of grog (crushed old pottery or crucible fragments) or coarse sand, plus a pinch of chopped grass or dung. The more grog, the better it resists heat shock.
  2. Form a cup 8–10 cm across and 7–9 cm deep with walls and base 1–1.5 cm thick. Pinch a pouring lip on one side. Make a few at a time.
  3. Dry in shade for a week, then fire them with your Pottery. Before every use, warm the crucible slowly beside the fire for 30 minutes — a cold or damp crucible thrown into a hot fire cracks.

Where to find it

Look for native copper in old basalt lava flows and in stream gravels below them, and for malachite and azurite as green and blue crusts on rusty, weathered outcrops — the gossans described in Finding and Identifying Ores. Test any green mineral by sprinkling it on hot coals: copper gives a bright green flame. Avoid grey, metallic copper ores at first: many contain arsenic or sulfur and need roasting (see Finding and Identifying Ores).

Method 1: Native copper, worked cold

If you find native copper, you can make tools today, with no furnace at all.

  1. Clean the lump. Break off rock with a hammerstone. Native copper is soft; rock is brittle and flakes away.
  2. Hammer it cold on your anvil stone with a smooth hammerstone. Strike firmly, turning the piece between blows, to draw it into a rod, a sheet or a blade shape.
  3. Feel it harden. After a few minutes of hammering, the copper stops moving under the blows and starts to spring back. This is work hardening: hammering tangles the metal's inner structure, making it harder but more brittle. Keep going and it will crack.
  4. Anneal it. Heat the copper in the fire to a dull red — just visible in shade, about 600–700 °C. You do not need to hold it there; as soon as the colour shows evenly, pull it out and drop it in water or let it cool in air. (Copper, unlike steel, becomes soft either way. Quenching also knocks off the black scale.) It is now soft again.
  5. Repeat hammer–anneal–hammer until the shape is finished.
  6. Finish cold. Do the last hammering cold, without annealing, especially along cutting edges and points. This leaves them as hard as copper can be — roughly twice as hard as annealed copper. Grind the edge sharp on a sandstone slab with water.
from the bellows Tuyereblast aimed down, 30–45° Charcoal heap8–10 cm over the crucible Cruciblethick clay with grog Ore + charcoal powderequal volumes Clay-lined pit30 cm wide, 20 cm deep yellow glow round the crucible: about 1,100–1,200 °C
Fig. 1 Smelting malachite in a crucible. The crucible sits buried in charcoal; the blast comes down on it from above.

Method 2: Smelting malachite in a crucible

This is how copper was probably first smelted: a small amount of rich ore, in a crucible, in a charcoal fire under a forced blast. It gives a few tens of grams at a time — enough for awls, beads and fish hooks — and teaches you everything you need for bigger furnaces.

Preparing the charge

  1. Pick the ore clean. Break it and keep only the green and blue parts. Grind them with a hammerstone on a flat stone to grains like coarse sand or rice (2–5 mm).
  2. Mix with charcoal. Take one volume of crushed ore and one volume of charcoal powder (1–3 mm, sieved through a coarse basket) and mix well. A good crucible charge is about 150–250 g of ore.

The hearth

  1. Dig a pit 30 cm across and 20 cm deep in dry ground, out of the wind, and line it with 3 cm of clay-sand mix.
  2. Set the tuyere at the rim of the pit, pointing down at about 30–45° so the blast will strike the crucible's top. The tip should sit about 5 cm from where the crucible's rim will be.
  3. Light a charcoal fire in the pit and let it burn for 20 minutes to dry and warm everything.

The smelt

  1. Bed the crucible. Push the hot coals aside, set the warmed crucible upright in the middle with 5 cm of glowing charcoal under it, and fill it with the ore–charcoal mix. Pack charcoal pieces round it and heap them 8–10 cm over the top.
  2. Blow. Start the bellows gently for 5 minutes, then at full steady rhythm. Within 15–20 minutes the charcoal round the crucible should glow orange-yellow. Green flames dancing on top are normal: copper is in the fire.
  3. Keep it at full heat for 45–60 minutes. Feed charcoal on top as it burns down; never let the crucible show through. You are looking for a yellow glow inside the heap — so bright it hurts to stare at.
  4. Check. Push a dry green stick into the crucible through the coals. Molten slag feels thick and sticky, like honey; you may feel harder beads at the bottom.
  5. Cool. Stop the blast, pull the crucible out with green-wood tongs onto dry sand, and let it cool. Do not pour yet.

Collecting the prills

  1. Break the cold contents out of the crucible. You will find a dark, glassy, bubbly lump of slag with green stains and, if you were lucky, a copper button at the bottom.
  2. Crush the slag to grit with a hammerstone on a flat stone. Copper prills do not shatter — they flatten into shiny pink flakes and beads. Pick them out, or pan the crushed slag in water (see Finding and Identifying Ores): the heavy copper stays behind.
  3. Save all prills from several smelts. When you have 50–200 g, melt them together (Method 4).

Tip Use a flux if the ore is dirty. If your ore has a lot of white quartz in it, mix in crushed red iron ore (hematite or roasted bog iron) — about one part to three parts of ore. Iron oxide and quartz melt together into a runny black slag at a much lower temperature, which lets the copper drops sink through.

Method 3: The bowl furnace

To make copper by the kilogram, scale up to a bowl furnace — a clay-lined pit with the ore and charcoal fed in from the top and blown from the side.

charge every 10–15 minutes from the bellows Tuyeresloping down about 30°,tip 10 cm above the bottom Chargeore + charcoal, 1 : 3 by weight Clay collar15–20 cm high Molten slagfloats on top Coppercollects in the bottom Clay-lined bowl30 cm wide, 25 cm deep
Fig. 2 A small bowl furnace in cross-section. Ore and charcoal go in from the top; copper drips down and collects in the bottom of the bowl, under the slag.
  1. Dig the bowl 30 cm across and 25 cm deep. Line it with 4–5 cm of clay mixed with sand and chopped grass. Build a low collar of the same mix around the rim, 15–20 cm high, to make a short shaft.
  2. Set the tuyere through the collar wall, sloping down at about 30°, its tip 2–3 cm inside the wall and aimed at the centre of the bowl, 10 cm above the bottom.
  3. Dry the furnace with a small wood fire for several hours (or a whole day). Wet clay in a hot furnace cracks and steams.
  4. Preheat. Fill with charcoal, light it, and blow gently for 30 minutes until the whole charge glows.
  5. Charge. Every 10–15 minutes, as the charcoal sinks, add a handful of ore (about 100–200 g, mixed with flux if needed) followed by enough charcoal to fill to the top. Over the smelt use roughly 3 parts charcoal to 1 part ore by weight. Keep the blast steady.
  6. Run it for 2–3 hours, putting in 1–2 kg of ore in total. Then add only charcoal for a final 20 minutes so the last copper melts down.
  7. Let it cool, then dig out the contents. You should find a heavy rounded cake of copper at the bottom of the bowl, covered with a crust of slag. Knock off the slag; crush it and pan it for prills.

A first furnace often gives only a third of the copper that is in the ore — a kilogram of good malachite might yield 150–300 g. With practice, and cleaner ore, you will do much better. Many failures are normal. Keep notes of each smelt.

Method 4: Melting and casting

Raw copper from smelting is spongy and full of slag. Melting it again in a clean crucible makes a solid, workable lump — and lets you cast it straight into a shape.

Green-wood tongs Cruciblecopper at yellow heat Pour fastone steady streamfrom one end Open mould on dry sandstone or fired clay: bone-dry, warm, sooted TOP VIEW OF THE MOULD flat axe ingot bar cavities 1–1.5 cm deep, sloping sides
Fig. 3 Pouring copper into an open mould. The mould must be bone-dry and warm; the pour is steady and fast, from one end.
  1. Make an open mould. Carve the shape of an ingot bar or a flat axe 1–1.5 cm deep into a block of soft, fine-grained stone (sandstone or soapstone), or press it into a slab of tempered clay and fire it. Make the walls sloped so the casting drops out.
  2. Dry and warm the mould beside the fire until it is too hot to hold and a drop of water on it sizzles away instantly. Smoke the cavity over a sooty flame (birch bark or resin) so the metal will not stick.
  3. Melt the copper in a crucible as in Method 2, but with only metal in it and a layer of charcoal on top. Blow until the charcoal glows yellow and the copper is a bright, swirling liquid — about 1,150–1,200 °C, a little above melting so it does not freeze in the pour.
  4. Skim the dross off with a dry green stick, then stir once with it. (The green wood releases gases that help remove oxygen from the copper; old smiths called this poling.)
  5. Pour. Lift the crucible with green-wood tongs, carry it the short distance to the mould at ground level, and pour in one steady stream from one end until the cavity is full.
  6. Wait a minute until the surface darkens, then tip the casting out. Quench it in water or let it cool.
  7. Finish. Cast copper is soft. Hammer it cold to shape and harden the edge, annealing when needed as in Method 1.

How to tell it worked

  • The scratch test. Real copper shows bright salmon-pink metal under a scratch or file; slag is black, glassy and brittle.
  • The hammer test. Copper flattens and bends without breaking. A lump that shatters is slag or matte (copper sulfide).
  • Weight. A copper lump is about three times heavier than a stone of the same size.
  • Colour on heating. Copper heated in air quickly goes rainbow-coloured, then black. A cast surface that is dull red-brown with green flame flickers on top during melting is normal.

Note Troubleshooting. Ore turned black but no copper → reduced but never melted: the fire was not hot enough. Use more blast, smaller pieces of charcoal, and keep at yellow heat longer. A grey, brittle, metallic lump → matte (copper sulfide). The ore had sulfur in it. Roast it first (see Finding and Identifying Ores). Copper beads trapped in thick, sticky slag → the slag did not melt. Add iron-oxide flux, or pick the ore cleaner. Casting full of holes → wet mould, or the copper soaked up gas. Dry the mould hotter, keep charcoal on the melt, pole it, and pour hotter. Crucible cracked → it was cold or damp when it went in, or needs more grog.

Dangers

Danger Water and molten metal explode. A drop of water under molten copper turns instantly to steam and throws the metal out in a burning spray. Pour only over dry ground or sand, into bone-dry warm moulds, with dry tools. Keep the quench bucket well away from the pour. Never pour when it is raining.

Danger Carbon monoxide and toxic fumes. Every smelt makes carbon monoxide. Many copper ores — especially grey ones — contain arsenic, which smokes white and smells of garlic; some contain lead or zinc. Smelt only in the open, stand upwind, and keep children away. Headache or dizziness: step away into fresh air.

  • Burns. Wear leather or wool, never anything that melts. Keep your feet covered. Lay out the path from fire to mould before you start, with nothing to trip over.
  • Eyes. Do not stare into a yellow-hot fire for long; look away often. Flying slag chips when crushing: turn your face away.
  • Failing crucibles. A crucible can crack in the tongs. Lift it low over sand, never over your feet.

What this unlocks

Copper plus tin gives Bronze: harder, easier to cast, and the material of an entire age. Copper with zinc gives brass. Better moulds, cores and lost-wax casting are in Metal Casting. Rolled or hammered thin it becomes Sheet Metal and Rolling; drawn through holes in a hard plate (see Iron and Brass Wire), it becomes Copper Wire, the foundation of electromagnets, the The Telegraph and the The Generator. The furnace skills here — bellows, tuyeres, slag, reduction — carry straight over to Iron (the Bloomery). Rock too poor to smelt can still give copper by leaching it with dilute acid (see Leaching, Solvent Extraction and Electrowinning).

How it was first done

The first metal objects were beads and awls hammered from native copper at sites in what is now south-east Turkey and northern Iraq, from about 9,000–8,000 BC; the people of Çayönü already annealed their copper. People in the Great Lakes region of North America later worked native copper on a large scale (from about 4,000 BC) without ever smelting it. Smelting copper from ore had begun by about 5,000 BC: at Belovode in Serbia, archaeologists have found slag and copper from malachite smelted around that date, and similar early smelting is known from Iran and Anatolia. For centuries most smelting was done in crucibles and small bowl furnaces like those described here. The copper axe carried by the "Iceman" who died in the Alps about 3,300 BC was cast from almost pure copper in a mould, then hammered to harden its edge.

Source: content/entries/metals/copper.md