Part 3 · Metals
Hammers, Pliers, Wrenches and Screwdrivers
The everyday steel hand tools of every workshop and household — claw, ball-pein and sledge hammers, pliers, pincers and wire cutters, spanners and adjustable wrenches, screwdrivers, punches and nail sets, crowbars, the bench vice and clamps — how to forge and fit each one, and how to heat-treat it so it neither bends nor shatters.
- Difficulty
- ●●●●●
- Time
- An afternoon to forge and handle a hammer; a day each for pliers, a spanner or a vice screw; a week for a leg vice
- Steps from zero
- 13 prerequisites →
This unlocks
—The full path from nothing — 13 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Hides and Leather
- Bellows
- Iron (the Bloomery)
- Blacksmithing
- Steel
- Hammers, Pliers, Wrenches and Screwdrivers
Do them roughly in this order. See it on the tech tree →
Why it matters
The first tools a smith makes are for the smith (Blacksmithing). The next go to everyone else: hammers and pincers for building (Timber Framing and Log Building), pliers for fence wire (Fences and Hedges), spanners for the nuts on carts, mills and engines (Screws, Nuts and Bolts), screwdrivers, punches, crowbars, and the vice and clamps that hold work still. A workshop stops without them.
Each has the same problem: the working part must be hard, or it dents and wears; the rest must be tough, or it snaps. A hammer face too soft mushrooms; too hard, it throws a steel chip into your eye. Getting this right is most of the craft.
How it works
Differential hardening. Make the tool of medium- or high-carbon Steel, harden only the working end, and temper each part to a different colour. The face, jaw or point is hard; the eye, joint, shank or handle stays tough and springy.
Temper colours (on a polished surface, slowly heated): pale straw 220 °C, dark straw 240 °C, brown 255 °C, purple 270 °C, blue 290–300 °C. The harder the blow the tool takes and the less sharp it must be, the bluer you temper it.
| Tool | Steel (carbon) | Harden | Temper the hard part to | Keep soft |
|---|---|---|---|---|
| Hand and claw hammer | 0.5–0.8% | both faces | dark straw to brown | eye, cheeks; claw blue |
| Sledgehammer | 0.5–0.7% | both faces | brown to purple | eye |
| Pliers and pincers | 0.5–0.8% | jaws | purple | joint, handles |
| Wire cutters | 0.8–1% | cutting edges | brown | joint, handles |
| Spanners and wrenches | 0.4–0.6% | whole tool | blue | — |
| Screwdriver | 0.6–0.8% | last 3 cm | purple to blue | handle end |
| Centre punch, nail set | 0.8–1% | point, 2 cm | purple | striking head |
| Crowbar, pry bar | 0.5–0.7% | both ends | blue | middle |
| Vice jaws | 0.8–1% (inserts) | faces | brown | body |
Running the temper. For a hammer: after hardening, polish the faces and the sides. Heat a thick iron bar red and push it through the eye, or hold the middle of the head over a small fire. Watch the colours creep out from the middle toward both faces. When brown reaches a face, dip that end in water; wait for the other. The middle ends up blue, the faces brown.
Leverage decides most proportions: a long handle on a short jaw multiplies force. A spanner is made only as long as it should be, so that one person cannot easily snap the bolt.
What you need
| Item | Notes |
|---|---|
| Forge tools | Anvil, tongs, hot chisel, an oval eye punch and eye drift; a striker for heavy heads (Blacksmithing) |
| Steel | Medium-carbon bar for heads, wrenches and bars; high-carbon for punches and cutters (Steel) |
| Finishing | Files, drill, tap and die (Files and Saws, Drills and Boring, Screws, Nuts and Bolts) |
| Wood | Seasoned, split hickory or ash wood for handles; oak or hornbeam for wedges and clamp jaws |
Where to find it
The best handle woods, hickory and ash, bend far before they break. Split blanks along the grain rather than sawing them, so the fibres run end to end, and season them a year (Basic Woodworking). Old cart springs and axles are salvaged steel of about the right carbon.
Hammers
The hammer head
All hammers are made the same way.
- Cut a block: about 25 × 25 × 100 mm for a 500 g head, 32 × 32 × 125 mm for 1 kg.
- Punch the eye a little toward the face end: at bright yellow, drive an oval eye punch halfway in from each side, dipping the punch often.
- Drift it open from both sides — about 18 × 30 mm for 500 g — so the eye is slightly hourglass-shaped. The wedged handle swells into the top flare and locks.
- Dress the cheeks back to shape over the drift.
- Shape the face very slightly domed (about 1 mm on a 25 mm face) with the edge chamfered 2–3 mm, so an off-square blow does not mark the wood and the edge does not chip.
- Normalise three times, harden each face end in turn, and temper as above.
| Hammer | Head weight | Handle | Use |
|---|---|---|---|
| Tack hammer | 100–200 g | 25 cm | small nails, upholstery |
| Claw hammer | 450–700 g | 30–35 cm | carpentry: driving and pulling nails |
| Ball-pein hammer | 100 g–1 kg (500 g common) | 30–38 cm | metalwork, riveting, punches |
| Lump (club) hammer | 1–2 kg | 25–28 cm | chisels on stone, driving stakes |
| Sledgehammer | 3–6 kg | 75–90 cm | splitting wedges, stakes, breaking stone, striking for a smith |
The claw hammer
- Draw the back of the head out into a flat tongue 6–8 cm long, tapering to 4–5 mm thick.
- Bend it down in a smooth curve, so the tip is in line with the bottom of the handle's eye.
- At a yellow heat, split it down the middle with a thin hot chisel from the tip to about 15 mm from the eye. Open the slot into a V: about 6 mm wide at the tip, narrowing to about 1.5 mm at the root, so it grips nail shanks of every size.
- File the inside of the V to two sharp edges and bevel the outer tips thin enough to slide under a nail head.
- Harden the face only; let the claw temper to blue, so it springs rather than snapping when you lever hard.
To pull a nail, slide the claw under the head, pull the handle back, and put a block of wood under the head for a long nail. A good claw grips a 3 mm nail without slipping and does not open up after a hundred nails.
The ball-pein hammer
The engineer's hammer. The back end is forged into a ball about 0.7 times the face diameter: draw it round, then shape it in a cupped swage or by filing. The ball spreads rivet heads (Nails, Rivets and Wire Fasteners) and stretches sheet metal (Sheet Metal and Rolling). Harden both ends.
The sledgehammer
A 3–6 kg head is too big to forge alone: a helper strikes while you turn the work, or use a water-powered hammer (Anvils, Trip Hammers and Power Hammers). The thrifty old way is a wrought-iron body with a steel plate 10–15 mm thick forge-welded onto each face. Temper the faces purple. The handle is 75–90 cm with a swell at the end so wet hands cannot lose it.
Handles and hafting
- Grain: growth rings on the end of the handle run in line with the head, as for axes (Axes, Chisels, Knives and Planes).
- Shape: oval, about 35 × 25 mm at a claw hammer's grip, slimmer just below the head so it flexes there and absorbs shock.
- Fit and wedge: shave to fit the eye tightly, drive on, saw flush, saw a slot two-thirds down the eye along its long axis, drive in a glued hardwood wedge, then an iron wedge across it. Never soak a loose handle in water: it swells for a day, then shrinks looser. Re-wedge it.
Pliers, pincers and wire cutters
Pliers are made like the smith's tongs in Blacksmithing, but finer and with a lap joint, so the jaws lie in one plane.
- Forge two halves from 12 mm square bar about 20 cm long: a jaw 3–4 cm long; a flat round boss about 22 mm across, forged to half the jaw's thickness so the two overlap; and a rein (handle) 12–15 cm long.
- Drill the bosses together (5–6 mm), set a hot soft-iron rivet, and work the joint while it cools so it moves freely.
- Jaws. Flat-nose: file both faces flat and cut fine cross grooves about 1 mm apart with a three-square file. Round-nose (for bending wire loops): file each jaw to a smooth tapering cone. Combination pliers add flat serrated tips, a rounded notch behind them for gripping round bar, and a pair of side cutters next to the joint.
- Harden the jaws and temper to purple; leave the joint and handles soft.
Pincers (18–25 cm) pull nails: their wide jaws meet across the front, and the rounded outside of one jaw is the fulcrum you roll them over.
Wire cutters have two hardened edges that meet exactly, unlike scissors, whose edges pass. Grind each edge to a wedge of 50–60°, like a small cold chisel. The two must touch along their whole length when closed: file and try, with soot on one edge to show where they touch. Side cutters have edges along the side of the jaws; end cutters (nippers) across the end, to cut wire flush with a surface. Handles should be 5–8 times longer than the distance from the joint to the cutting edge. Temper the edges brown. Cutting hardened spring wire notches any edge; use the corner of a file and break it instead.
Spanners and wrenches
The open-ended spanner
A spanner (or wrench) turns a nut or bolt head by its flats.
- Jaw opening = the nut's width across the flats + 0.1–0.3 mm. Too tight, it will not go on; too loose, it rounds the corners off the nut.
- Jaws angled at 15° to the handle. In a tight space, turn the nut, flip the spanner over, and you can turn it again — it moves in 30° steps.
- Length about 10–15 times the opening for small sizes (a 13 mm spanner is about 16–18 cm long), less for big ones. That limits the force so a person cannot easily strip a small bolt.
- Head thickness about 0.4 times the opening.
Making one: forge a medium-carbon bar into a handle with a round, flat paddle at the end about 2.5 times the jaw opening across. Punch or drill a hole the size of the opening in the middle of the paddle, then cut out the mouth from the hole to the edge with a hot chisel at 15° to the handle line. File the jaws parallel until a gauge — a hardened square bar of exactly the right size, or a good nut — slides in with no shake. Stamp the size on it. Temper the whole spanner blue: hard jaws crack, soft jaws spread.
Ring spanners have a hexagon filed into a closed ring and cannot slip; box spanners are tubes hammered hexagonal over a mandrel. All need nuts made to fixed sizes (Screws, Nuts and Bolts).
The adjustable wrench
The monkey wrench is the one to make first: a bar 20 × 12 mm with a fixed jaw forged at right angles at its end; a second jaw with a rectangular hole filed to slide on the bar without rocking; and below it, a thread cut on a rounded part of the bar (Screws, Nuts and Bolts) with a knurled nut that pushes the sliding jaw up. File both jaw faces square to the bar. It fits nuts up to about 5 cm.
The adjustable spanner (crescent type) has its sliding jaw in a slot in the head, moved by a small worm — a screw that turns in a pocket and engages a row of teeth (a rack) cut on the jaw. It is slimmer and handier but needs accurate machining (Machine Tools).
Always pull an adjustable wrench so the force goes into the fixed jaw, and tighten it snugly on the nut before you pull.
Screwdrivers
A screwdriver must fill the slot. Its proportions:
- Tip thickness exactly the slot width: it should fit snugly.
- Tip width equal to the screw head's diameter, or a little less, so it does not scar the wood beside the head.
- Flanks nearly parallel for the last 2–3 mm, then flaring. A blade ground to a sharp wedge rides up and out of the slot (it cams out) and chews the screw.
- Shank round, 5–8 mm, 7–25 cm long, with a flattened tang driven into the handle, or a square section near the handle so a spanner can help turn it.
- Handle of hardwood, oval or fluted, 10–12 cm long, with a brass or iron ferrule.
Forge the tip flat, file it to fit a real slot, harden the last 3 cm and temper purple-blue — too soft twists, too hard chips. Make three or four sizes.
Punches and nail sets
- Centre punch: a bar of high-carbon steel 10–12 mm thick and 10–12 cm long, the point ground to 90°. A dent from it guides a drill so it starts exactly where you want (Drills and Boring, Machine Tools).
- Prick punch: the same with a 30–60° point, for fine layout marks.
- Pin punch (drift): a parallel tip, flat-ended, to drive pins and rivets out of holes.
- Nail set: a tapered tip 1.5–3 mm across with a small cup drilled in the end, to sit on a nail head and drive it 2–3 mm below the surface, ready to be filled.
Harden the point 2 cm and temper to purple. Leave the striking end soft and chamfered. Every punch and chisel head spreads into a mushroom over time. Grind it off as soon as it forms.
Crowbars and pry bars
A crowbar (wrecking bar) is a long steel lever. Forge it from round or hexagonal medium-carbon bar 20–25 mm thick and 60–120 cm long. One end is a gooseneck: bent into a tight curve with a radius of about 5 cm, flattened and split into a claw for nails, like a hammer claw. The other end is a chisel point, bent 10–15° so it can be pushed into a crack and then levered. A 1 m bar with its fulcrum 5 cm from the tip multiplies your force about twenty times (Simple Machines).
A pry bar is a flat bar 30–40 cm long, about 30 × 6–8 mm, with a thin bevelled end slotted for nails and slightly bent, for prising boards apart without splitting them.
Harden both ends and temper blue; leave the middle as forged. A bar must bend before it breaks, never snap.
The bench vice
The smith's leg vice takes hammering. Details of its use are in Machine Tools. Its parts:
- Back jaw and leg: a bar of iron about 50 × 25 mm standing on the floor, jaws at elbow height (about 1 m), so hammer blows go into the ground. Bolt it to the bench with a forged mounting plate.
- Front jaw and leg: the same, joined to the back leg by a pivot 15–20 cm above the floor.
- Jaw faces 10–15 cm wide: weld on high-carbon steel strips, cut crossed grooves, harden and temper brown.
- The screw: steel 25–32 mm across with a square or rounded thread of about 6–8 mm pitch, cut by hand or on a lathe (Screws, Nuts and Bolts), with a sliding tommy bar through its head.
- The box (nut): the traditional way avoids cutting an internal thread. Wind a square iron rod round the finished screw as a tight spiral, slide the spiral off, push it into an iron tube that fits round it, and braze it in place (Soldering and Brazing). The spiral is the thread.
- The spring: a flat leaf spring between the legs (Springs) that opens the jaws as you unscrew.
The swinging jaw is parallel at only one opening; the parallel vice comes later (Machine Tools). Wood vices are in Planes, Drawknives and Woodworkers' Tools.
Clamps
- Wedges are the first clamp: two cleats nailed to a board, the work between them, and a pair of folding wedges (two identical wedges, point to butt) tapped together.
- Handscrew: two hardwood jaws about 30 × 5 × 5 cm joined by two wooden screws 20–25 mm across (Screws, Nuts and Bolts). Turning the screws by different amounts lets the jaws grip work that is not parallel.
- G-clamp: forge flat bar 25 × 10 mm into a C (a T-section is stiffer), upset a boss at one end, drill and tap it 10–16 mm, and fit a screw with a tommy bar and a swivel pad peened loosely onto its tip so it sits flat on the work. A 100 mm clamp has a throat about 50–60 mm deep. Normalise only.
- Bar clamp (sash cramp): a long bar with a screw head at one end and a stop pinned through holes, for glueing wide panels (Furniture).
How to tell it worked
- File test: a file skates on hammer faces, jaw tips and punch points, but bites eyes, joints, handles and the middle of a crowbar.
- Hammer: fifty blows on soft iron — no dent, no chip.
- Spanner: measure the opening before and after a hard pull; it must not spread or rock on the nut.
- Pliers and cutters: jaws meet along their length with no light between; cutters snip 2 mm iron wire cleanly.
- Screwdriver: drives a tight screw without twisting, chipping or jumping out.
- Crowbar: under your full weight it may flex and spring back, but must not stay bent or crack.
Note Troubleshooting. Hammer face dents → face not hard; reharden and temper only to straw-brown. Face chips → too hard; temper more. Head comes loose → eye not flared, wedge too small, or the handle shrank. Re-wedge; drift the eye's top flare wider. Handle breaks just below the head → wrong grain orientation, or a misplaced blow. Make a new handle with the rings in line with the head. Pliers stiff → rivet too tight. Heat the joint red and work it. Spanner rounds off nuts → jaws too wide or not parallel. Re-file to a gauge. Screwdriver cams out → tip ground to a wedge. Regrind with parallel flanks.
Dangers
Danger Flying steel. A hardened hammer face struck on another hardened face — another hammer, an anvil horn's tip, a hard punch head — can shed a sharp chip that flies like a bullet and can blind or kill. Never strike two hammers together. Grind every mushroomed punch and chisel head. Wear eye protection when striking hardened tools, and keep bystanders out of line.
Warning Loose heads and slipping tools. A head that flies off a sledge on the swing can kill a bystander: check the wedge every day. A crowbar or spanner that slips throws you off balance — pull toward you rather than push, keep your knuckles out of the path, and do not stand on a bar under load.
- Crushing: a vice screw multiplies force hundreds of times; keep fingers out of the jaws.
- Hot steel looks exactly like cold steel (Blacksmithing).
- Striking in pairs: agree who calls each blow; the holder uses tongs, never hands.
What this unlocks
With hammers, pincers and punches, carpentry and building go fast (Timber Framing and Log Building, Doors, Windows and Joinery, Furniture). With spanners and screwdrivers, machines can be bolted together and taken apart for repair (Screws, Nuts and Bolts, Precision and Interchangeable Parts) — a The Bicycle, a The Sewing Machine or an The Motor Vehicle is assembled with little else. The vice and clamps are the start of the fitter's bench (Machine Tools) and of fine woodwork.
How it was first done
Hammerstones are the oldest tools known: struck stones about 3.3 million years old have been found at Lomekwi in Kenya (Stone Tools). Hafted stone hammers and mauls followed in the Stone Age. Smiths' tongs and hammers of bronze and iron appear with metalworking; Roman carpenters had iron claw hammers, pincers and nail-pulling claws much like ours. Screwdrivers appear in Europe in the 15th century, at first for the screws in armour and gunlocks. Wrenches for nuts became common with bolts in the 17th–18th centuries. The monkey wrench was patented by Loring Coes in Massachusetts in 1841, and the slim adjustable spanner with a worm was developed by Johan Petter Johansson in Sweden around 1891. Cross-head screws spread from the 1930s.
Source: content/entries/metals/hand-tools.md