◆ Rebuild

Part 8 · Chemistry

Synthetic Rubber Works (Overview)

Where rubber trees will not grow, or there are too few of them, rubber can be built from oil, gas or alcohol. Butadiene and styrene stirred in soapy water join into long chains that make SBR, the rubber of most tyres; related works make butyl for inner tubes, EPDM for weather seals and nitrile for oil seals. How the works runs in outline, how to compound synthetic rubber with carbon black, press it into sheet, build a tyre and an inner tube, and keep the people safe.

Difficulty
●●●●●
Time
Years and a chemical industry to build a works; a day to compound a batch; 20 minutes to press-cure a sheet; a day to build and cure a few tyres by hand
Steps from zero
46 prerequisites →

You need first

Silicones and Synthetic RubbersPetroleum and Refining

This unlocks

—
The full path from nothing — 46 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Simple Machines
  8. Hunting and Trapping
  9. Basic Woodworking
  10. Charcoal
  11. Pottery
  12. The Kiln
  13. Quarrying and Cutting Stone
  14. Rubber
  15. Hides and Leather
  16. Bricks
  17. Lime
  18. Salt
  19. Mining and Tunnelling
  20. Lye and Potash
  21. Fermentation
  22. The Wheel and Axle
  23. Firebrick and Refractories
  24. Glass
  25. Bellows
  26. Saltpeter
  27. Distillation
  28. Gears
  29. Coal and Coke
  30. Iron (the Bloomery)
  31. Copper Smelting
  32. Sulfuric Acid
  33. Coal Tar Chemicals
  34. Laboratory Glassware
  35. The Waterwheel
  36. Blacksmithing
  37. Hydrochloric Acid
  38. Organic Synthesis and Fine Chemicals
  39. Magnets
  40. Steel
  41. Copper Wire
  42. Petroleum and Refining
  43. The Generator
  44. The Electric Arc Furnace
  45. Pure Silicon
  46. Silicones and Synthetic Rubbers
  47. Synthetic Rubber Works (Overview)

Do them roughly in this order. See it on the tech tree →

Why it matters

Natural rubber grows only in a narrow belt of warm, wet country, and a plantation takes six or seven years to tap. A community far from that belt, or needing more than its trees give, must make rubber. Germany did so in 1914–18, and the United States in 1942 built a synthetic rubber industry from almost nothing in three years.

Synthetic rubbers also do things natural rubber cannot. SBR, made from butadiene and styrene, wears more slowly in a tyre tread and is cheap; it is now most of the rubber in the world. Butyl holds air eight to ten times better, so it makes inner tubes and the airtight lining of tubeless tyres. EPDM shrugs off sunlight, ozone and steam for decades, for door and window seals, roof sheets and radiator hoses. Nitrile and neoprene resist oil and petrol (Silicones and Synthetic Rubbers).

This chapter is an overview. A synthetic rubber works is a full chemical plant with gases under pressure, refrigeration and continuous control (Process Controllers and Control Valves), and belongs late in rebuilding, after Petroleum and Refining refining or a large Fermentation industry. What a workshop can do with traded raw rubber, compounding, moulding and building tyres, is given in full.

How it works

Rubber is long chains. Every rubber is made of enormously long, coiled molecules that straighten when stretched and curl back when let go. Natural rubber's chains are built from isoprene, a small molecule of five carbon atoms. Synthetic rubbers are built from similar small molecules (monomers), joined end to end by polymerisation (Petrochemicals and Modern Plastics, Organic Synthesis and Fine Chemicals).

The monomers.

Monomer Boils at Made from Gives
Butadiene (4 carbons, 2 double bonds) −4 °C (a gas) Cracked oil gases, butane, or alcohol SBR, polybutadiene, nitrile
Styrene 145 °C Benzene and ethylene SBR (with butadiene)
Isobutylene −7 °C Cracked oil gases Butyl
Ethylene, propylene −104, −48 °C Cracked oil or gas EPDM
Acrylonitrile 77 °C Propylene, ammonia and air Nitrile
Chloroprene 59 °C Acetylene or butadiene, with chlorine Neoprene

Emulsion polymerisation. Butadiene and styrene stirred hard into soapy water break into tiny droplets. A starter dissolved in the water makes reactive fragments that enter the soap clusters and set chains growing, each adding thousands of monomer molecules. The result is a milky latex, very like a rubber tree's. The water carries away the heat and keeps the thick rubber flowing.

Stopping in time. Run to the end, the chains cross-link into a useless gel. So a shortstop chemical stops it at about 60–72 % conversion and the unused monomer is recovered. A little modifier (a mercaptan, a sulfur compound) keeps the chains short enough to mill.

Hot and cold rubber. The first SBR was made at 50 °C. From 1947 a more active starter allowed 5 °C ("cold rubber"), whose more regular chains wear better in tyres.

SBR is weak alone. Natural rubber stiffens and strengthens itself when stretched, as its regular chains line up into tiny crystals. SBR's irregular chains cannot. Pure cured SBR tears at about 2–3 MPa, a tenth of natural rubber. Milled with carbon black (Lampblack and Carbon Black), it reaches 20–25 MPa and wears better than natural rubber. Every SBR article is filled.

What you need

For Item See
The works Monomer plants; cooled pressure reactors; flash tanks and stripping column; coagulation tanks, dryer, baler; soap, starter, modifier, shortstop, antioxidant, salt and acid Distillation, Pressure Vessels and Valves, Ice and Refrigeration, Soap, Sulfuric Acid
Compounding Two-roll mill (rolls 15–40 cm across, water-cooled); scales; carbon black; zinc oxide; stearic acid; sulfur; accelerator; process oil; wax Lampblack and Carbon Black, Zinc and Brass, Sulfur
Moulding Heated hydraulic press of about 20 tonnes; steel picture-frame mould; tyre moulds; curing bladders Hydraulic Presses and Rams, Metal Casting
Tyres Building drum; cord fabric of cotton, rayon or nylon; bronze-coated steel bead wire Spinning and Weaving Cloth, Rayon and Nylon, Iron and Brass Wire

Making the monomers (in outline)

Butadiene from alcohol. The oldest route, and the one open to a country with sugar or grain but no oil. Ethyl alcohol vapour (Fermentation, Spirits, Sake and Liqueurs) passes over a catalyst of magnesia with silica or zinc oxide at about 400–450 °C. It loses water and hydrogen and pairs up into butadiene. Roughly 2.5–3 tonnes of alcohol make a tonne of butadiene. Sergei Lebedev's plants in the Soviet Union worked this way from 1932, and so did most American butadiene in 1943–44.

Butadiene from oil. Steam-cracking naphtha for ethylene (Petrochemicals and Modern Plastics) leaves a four-carbon gas fraction rich in butadiene. Its neighbours boil within a few degrees of it, so it is separated by extractive distillation, with a solvent such as furfural (from oat husks or corn cobs) fed down the column to hold the butadiene back (Distillation).

Styrene. Benzene and ethylene join over aluminium chloride to give ethylbenzene, which is passed with a large excess of steam over an iron oxide catalyst at about 600–630 °C, losing hydrogen. Styrene is distilled under vacuum at low temperature with an inhibitor in the still, because heated styrene polymerises by itself into a solid lump.

Both monomers are stored cold, under nitrogen, with a trace of inhibitor washed out with caustic soda just before use (Lye and Potash).

The SBR works

Butadiene Styrene Soapy water, starter, modifier Chain of 10–12 stirred reactors cooled to 5 °C or 50 °C Shortstop Flash tanks butadiene boiled off and reused styrene stripped and reused Steam stripper steam latex Latex tank antioxidant, oil brine acid Coagulation wet crumb forms Wash and squeeze Dryer hot air, 80–100 °C Baler 35 kg bales
Fig. 1 An SBR works in outline. Butadiene, styrene, soapy water, starter and modifier are pumped through a chain of cooled, stirred reactors. Shortstop is added when about 60 % has reacted. Unused butadiene is flashed off and styrene steam-stripped, both returning to the feed. Antioxidant is added, the latex is coagulated with salt and acid into crumb, washed, dewatered, dried and pressed into bales.

The wartime American standard recipe for hot rubber, in parts by weight:

Ingredient Parts
Butadiene 75
Styrene 25
Water 180
Soap 5
Potassium persulfate (starter) 0.3
Dodecyl mercaptan (modifier) 0.5

At 50 °C for about 12 hours it reaches about 72 % conversion. Cold rubber uses rosin soap and a redox starter (an organic peroxide with a trace of iron salt) at 5 °C, stopped at about 60 %.

  1. React. The ingredients flow through a chain of 10–12 stirred reactors of 15–40 m³, glass-lined or stainless, cooled by jackets and coils that hold the temperature within a degree (Process Controllers and Control Valves). Conversion is followed by drying and weighing samples.
  2. Shortstop is pumped in at the target conversion.
  3. Recover monomer. In flash tanks, at low pressure then vacuum, the butadiene boils off to be compressed and reused; styrene is steam-stripped in a tray column.
  4. Antioxidant (1–1.5 parts) is stirred in, and for tyre grades often 25–37 parts of oil ("oil-extended" SBR).
  5. Coagulate with brine, then dilute sulfuric acid to about pH 3–4, which also turns the soap into fatty acid that later helps the cure. The rubber comes out as wet crumb, like cottage cheese.
  6. Wash, squeeze and dry the crumb in hot air at 80–100 °C, and press it into bales of about 35 kg.

Each batch is tested for Mooney viscosity (the stiffness of the raw rubber against a disc rotating in it at 100 °C, about 45–55 for tyre grades), or simply milled beside a good reference sample.

Other synthetic rubbers (in outline)

  • Butyl (IIR): isobutylene with 1.5–3 % isoprene, polymerised in methyl chloride with aluminium chloride at about −100 °C, so fast that it is over in seconds. It is very airtight, absorbs shocks, and resists ozone and acids. Inner tubes, tyre inner liners, curing bladders, pharmaceutical stoppers. With a little bromine or chlorine added (halobutyl) it bonds to other rubbers in a tyre.
  • EPDM: ethylene and propylene with a few per cent of a third monomer that leaves points for sulfur to bridge, joined in solution with a vanadium catalyst (a Ziegler–Natta catalyst). Lasts decades in sun and weather and in hot water; swells in oil. Window and door seals, roofing sheet, radiator hoses, electrical insulation.
  • Polybutadiene and synthetic polyisoprene: made with the same catalysts. Polybutadiene is springy and hard-wearing, blended 20–40 % into treads; polyisoprene is almost identical to natural rubber.
  • Nitrile and neoprene, for oil and weather: see Silicones and Synthetic Rubbers.

Compounding synthetic rubber

Raw synthetic rubber, like raw natural rubber, is not yet useful. It must be compounded: mixed with fillers and curing chemicals, then shaped and cured (Rubber gives the cure in the sand bath). A phr is a part by weight per hundred parts of rubber.

A tyre-tread compound:

Ingredient phr Purpose
SBR (or 70 SBR + 30 polybutadiene) 100 The rubber
Carbon black, a fine reinforcing grade 50 Strength and wear
Process oil (aromatic or naphthenic) 5–10 Easier mixing, softness
Zinc oxide 3 Activates the cure
Stearic acid 2 Activates the cure, helps mixing
Antioxidant / antiozonant 1–2 Slows ageing and cracking
Paraffin wax 1–2 Blooms to the surface against ozone (Waxes: Beeswax, Plant Waxes and Paraffin)
Sulfur 1.75 Cross-links
Accelerator (a sulfenamide) 1 Fast, safe cure

SBR needs less sulfur and more accelerator than natural rubber, and cures more slowly. Avoid accelerators that release nitrosamines (those made from secondary amines such as dimethylamine); they cause cancer.

Two-roll mill, end viewPicture-frame mould, opened out Carbon black added a little at a time Bank Front roll rubber bands round it Back roll 10–25 % faster Cooling water inside keep below 70 °C Trip bar stops the rolls Heated platen 160 °C Top plate Compound 5–10 % extra Frame 2 mm thick, 150 mm opening Bottom plate Platen About 10 MPa
Fig. 2 Compounding and moulding. On the two-roll mill, rubber bands round the front roll and powders are added to the bank of rubber in the nip; the back roll turns faster and shears the mix. A trip bar across the front stops the rolls. Right, a picture-frame mould: a steel frame between two flat plates, overfilled with compound and pressed between heated platens to make a flat sheet.

On the two-roll mill

  1. The mill. Two chilled cast-iron or hardened steel rolls turning towards each other, the back roll 10–25 % faster so the rubber is sheared, water-cooled inside (The Blast Furnace and Cast Iron). Rolls 15 cm across and 30 cm long do 1–2 kg batches.
  2. Band the rubber. At a gap of about 2 mm, SBR bands round the front roll as a smooth skin within minutes; it needs far less breaking down than natural rubber.
  3. Add the dry ingredients in order: zinc oxide, stearic acid and antioxidant first; then carbon black a little at a time, with the oil, into the bank (the rolling bead of rubber in the nip). Keep the rolls below about 70 °C by the water flow.
  4. Cut and fold. Cut three-quarters across the band with a knife on alternate sides and fold it back, a dozen times, so the mix is even. No grey streaks or specks of black may remain.
  5. Sulfur and accelerator last, at the end, with the rolls cool, in no more than 3–5 minutes, so the compound does not start curing on the mill (scorch).
  6. Sheet off at about 5 mm and cool on a clean table. Label each batch. Compound keeps for weeks in a cool place.

A large works mixes 100–250 kg at a time in a closed internal mixer (a Banbury) and sheets it on a mill.

The synthetic rubber sheet

A flat sheet of cured rubber is the first object to make, the stock for gaskets, washers, pump diaphragms, valve seats, mats and test pieces (Packing, Gaskets and Seals).

  1. The mould. A picture-frame mould: a steel frame as thick as the sheet wanted (1, 2, 3 or 6 mm), with an opening say 150 × 150 mm, between two flat, polished steel plates 6–10 mm thick. Dust or wipe the plates with a little soapy water or talc so the rubber releases.
  2. Charge. Cut compound to fill the frame with 5–10 % extra by weight: weight = length × width × thickness × density (filled SBR is about 1.15 g/cm³). A 150 × 150 × 2 mm sheet needs about 52 g; charge 56 g.
  3. Press. Put the stack between platens of a hydraulic press heated to 160 °C (water dropped on them spits and dances; better, a thermocouple, Thermocouples and Thermoelectricity). Close and apply pressure, open briefly once or twice (bumping) to let trapped air out, then hold at about 10 MPa on the cavity: a 20-tonne press on a 150 mm square.
  4. Cure time. About 15–20 minutes for 2 mm at 160 °C with the compound above; add about 5 minutes for each extra 2 mm. Find the right time once by curing sheets for 10, 15, 20 and 30 minutes and testing them.
  5. Demould hot, peel the sheet out, trim the flash (the thin fin squeezed out round the edge), and let it rest a day before testing.

Without a press, clamp the plates with heavy G-clamps and cure in a sand bath or oven as in Rubber; expect more bubbles.

Good versus bad sheet. A good sheet is evenly thick to ±0.1 mm, glossy, free of bubbles and blisters, black right through with no streaks, and returns at once from a sharp fold with no white crease. A dumbbell cut from it stretches to four to six times its length before breaking. A sheet that is sticky or soft was undercured; one that is hard and cracks on folding, overcured or overloaded with black. Small bubbles mean trapped air or damp ingredients; a blistered surface means it was demoulded too early.

The tyre

A tyre is the biggest use of synthetic rubber. Building one by hand is within reach of a careful workshop with moulds.

Tread SBR and carbon black Steel belts radial tyres only Carcass ply rubber-coated cord fabric, turned up round the bead Inner liner butyl: keeps the air in Sidewall soft, flexes, resists ozone Air Bead hoop of brass-coated steel wire Rim Grooves
Fig. 3 A tyre in cross-section. The tread of hard-wearing SBR compound touches the road; the sidewalls are softer and resist ozone. Inside, layers of rubber-coated cord (the carcass) wrap round two bundles of steel wire (the beads) that hold the tyre on the rim. In a radial tyre, steel-cord belts lie under the tread. A thin layer of butyl, the inner liner, keeps the air in.

The parts.

  • Tread: SBR compound as above, 8–10 mm deep on a car tyre, with grooves to clear water.
  • Sidewalls: a softer compound with more antiozonant, often with natural rubber or EPDM, that flexes millions of times without cracking.
  • Carcass: one to four plies of cord fabric (cotton, then rayon, then nylon or polyester), the cords coated on both sides with a thin rubber skim on a calender (a three-roll machine that presses rubber into fabric).
  • Beads: a bundle of bronze- or brass-coated steel wires, about 1 mm each, wound into a hoop that fits the rim exactly (Iron and Brass Wire). Brass coating bonds to rubber; bare steel does not.
  • Inner liner: a thin sheet of halobutyl, for tubeless tyres.
  • Belts (radial tyres): two layers of steel cord at about 20° to the centre line under the tread.

Building.

  1. On a collapsible drum a little wider than the tyre, lay the inner liner, then the first ply. In a cross-ply (bias) tyre, the cords of each ply run at about 35–40° to the centre line, alternate plies crossing. In a radial tyre, the carcass cords run straight across, at 90°.
  2. Set the beads at each edge and turn the plies up round them, rolling out all air with a hand stitcher (a small toothed wheel).
  3. Add sidewall strips, (belts for a radial), and the tread strip on top, each splice overlapping a few millimetres and rolled down firmly.
  4. Collapse the drum and lift off the green tyre: a flat, uncured band.

Curing. The green tyre goes into a two-part steel mould engraved with the tread pattern, heated to about 170 °C. A rubber bladder inside is inflated with steam or hot water at 15–25 bar, pressing the tyre into the mould. A car tyre cures in about 10–15 minutes, a truck tyre in about an hour. A bicycle tyre, one ply of fabric with a thin tread, cures in a few minutes in a simple ring mould.

Good versus bad tyre. Check every tyre: no blisters or bulges (trapped air), no exposed or wavy cords, beads evenly seated, tread full depth. Mount it, inflate it in a steel cage to 1.5 times working pressure, and spin it: it should run true within about 1 mm. Cut one tyre from every batch in half to see that the plies are bonded with no gaps.

The inner tube

An inner tube is a ring of butyl rubber with a valve. Before tubeless tyres it held the air in every tyre, and it still does in bicycles, wheelbarrows and carts (The Bicycle).

  1. Extrude butyl compound through a die as a seamless tube, walls 1–2 mm for a bicycle, 2.5–4 mm for a car or cart, talc-dusted inside.
  2. Cut to the tyre's inside circumference plus a few centimetres, punch a hole, and press on a valve with a rubber base pad (The Bicycle has the valve).
  3. Splice the square-cut ends, softened with solvent (Ether, Acetone and Solvents), butted and pressed.
  4. Cure in a ring mould at about 170 °C for 5–10 minutes, with steam inside.
  5. Test under water at working pressure for five minutes: no bubbles. Butyl holds air for months; natural rubber tubes lose it in weeks.

How to tell it worked

  • Identify a rubber. Hold a strip in a flame. Natural rubber and SBR burn smoky with a sweetish rubber smell; SBR also smells of styrene, like hot plastic. Touch a hot copper wire to a rubber and then put it in a flame: a green flame means chlorine, so neoprene (the Beilstein test). Silicone leaves a white ash of silica.
  • Oil test. Weigh a piece, soak it in kerosene for three days, reweigh. Nitrile gains less than about 20 %; SBR, natural rubber, butyl and EPDM swell to double or more.
  • Weather test. Bend strips into loops, tie them, and leave them in sun on a roof. SBR and natural rubber without antiozonant crack within weeks; EPDM and butyl last for years.
  • Hardness. Tread compounds are about 60–70 Shore A; keep reference samples and compare by thumbnail.

Note Troubleshooting. Compound crumbles and will not band on the mill → gap too wide, rubber too cold, or too much black added at once. Close the gap; add black slowly. Compound goes stiff on the mill → scorch: rolls too hot, or curatives added too early. Discard it and keep curatives till last. Sheet weak and sticky → undercured, or too little sulfur. Cure longer. Bubbles in moulded parts → damp powders or trapped air. Dry the black; bump the press. Tyre separates between plies → contaminated or old ply skim, too little rolling, or plies laid too dry. Keep surfaces clean and tacky; stitch harder.

Dangers

Danger Butadiene is a heavy, highly flammable gas that pools in pits and drains, and it causes cancer. In contact with air it slowly forms explosive peroxides, and in pipes and tanks it can grow a hard "popcorn" polymer that swells enough to split steel. Keep it cold, inhibited and under nitrogen; never let air into the system; inspect for popcorn growth. Acrylonitrile is poisonous through the skin and lungs. Styrene vapour is harmful and its storage can run away if the inhibitor is used up. A runaway emulsion reactor can burst. These belong only in a properly built works with gas detectors, relief valves and trained staff.

Danger Mills and presses take hands and arms. The nip of a two-roll mill draws a glove, sleeve or hand in and crushes it. Every mill must have a trip bar or body bar across the front, at waist to chest height, that stops the rolls within a fraction of a turn, and an emergency stop the operator can reach with the knee. Never reach over the rolls or feed close to the nip with fingers; push rubber in with a wooden stick. Curing presses close with tonnes of force and are at 160–180 °C.

  • Tyre inflation kills. A tyre or rim that fails during inflation explodes with enough force to kill. Inflate new tyres and any multi-piece rim in a steel cage, with a clip-on chuck and a long hose, standing to one side.
  • Carbon black dust: closed bags and dust extraction (Lampblack and Carbon Black). Curing fumes: ventilate presses.
  • Tyre dumps that catch fire burn for months, poisoning air and water; store old tyres in small, separated stacks.

What this unlocks

Synthetic rubber frees the tyres of the The Bicycle, The Motor Vehicle, The Tractor and Gliders and Aeroplanes from the plantation. Butyl gives inner tubes and stoppers for medicine vials (Syringes and Hypodermic Needles); EPDM, lasting seals for Roofs and heating systems; nitrile, seals that stand oil (Hydraulic Presses and Rams); rubber sheet, the diaphragms of Process Controllers and Control Valves valves.

How it was first done

Charles Greville Williams distilled isoprene from natural rubber in 1860; Fritz Hofmann at Bayer patented a synthetic rubber from isoprene in 1909; and blockaded Germany made a few thousand tonnes of poor "methyl rubber" in the First World War. Sergei Lebedev polymerised butadiene in 1910, and from 1932 the Soviet Union made sodium-polybutadiene from alcohol in large plants at Yaroslavl and elsewhere. At IG Farben, Walter Bock and Eduard Tschunkur made butadiene–styrene rubber, Buna S, in 1929, and Erich Konrad and Tschunkur nitrile rubber, Buna N, patented in 1934. DuPont announced neoprene in 1931, and William Sparks and Robert Thomas of Standard Oil invented butyl in 1937. When Japan took the rubber plantations of Southeast Asia in 1942, the United States built about fifty plants in under three years and was making roughly 70,000 tonnes of synthetic rubber a month by 1945, mostly GR-S, its name for SBR. Cold rubber followed in 1947, and the Ziegler–Natta catalysts of the 1950s gave synthetic polyisoprene, polybutadiene and EPDM. The air-filled tyre was patented by Robert William Thomson in 1845 and reinvented by John Boyd Dunlop for a bicycle in 1888; Michelin sold the first steel-belted radial tyre in 1949.

Source: content/entries/chemistry/synthetic-rubber.md