◆ Rebuild

Part 8 · Chemistry

Potassium Permanganate

Fuse black manganese ore with caustic potash in air or with saltpeter and you get a green melt; dissolve it, bubble carbon dioxide through, and it turns a startling purple. The dark crystals that grow from it are potassium permanganate — a strong oxidiser for disinfecting skin, cleaning iron and bad smells out of well water, testing water for pollution, and measuring iron and other substances by colour alone.

Difficulty
●●●●●
Time
An afternoon to roast or fuse the melt; a day to convert and settle; a day or two to crystallise
Steps from zero
5 prerequisites →

You need first

Lye and PotashThe Kiln

This unlocks

—
The full path from nothing — 5 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. The Kiln
  5. Lye and Potash
  6. Potassium Permanganate

Do them roughly in this order. See it on the tech tree →

Why it matters

A few purple crystals of potassium permanganate dissolved in water make one of the most useful household and laboratory chemicals there is:

  • Skin and wound soaks. A pale pink solution dries up weeping, oozing skin, blisters and fungal infections of the feet, and cleans dirty ulcers (Wound Care and Antiseptics).
  • Water treatment. It turns dissolved iron and manganese — which stain laundry and make water taste of metal — into solids that can be filtered out, and destroys the rotten-egg smell of sulfur wells (Water Treatment for a Town, Wells and Cisterns).
  • A pollution test. A drop in clean water stays pink for hours; in water fouled by sewage or rotting matter it fades to brown in minutes (Identifying Substances).
  • Measuring. Its own colour shows the end of a titration with no indicator. It measures iron in ores, the strength of hydrogen peroxide (Hydrogen Peroxide and Oxygen Bleach), and the organic load in water.
  • Smaller jobs. It stains wood a warm brown, oxidises other chemicals in the laboratory, and, soaked into fired clay granules, absorbs the gas fruit gives off as it ripens, so stored fruit keeps longer (Preserving Food).

It needs only three things you can already make: black manganese ore, caustic potash from wood ash (Lye and Potash), and a hot fire or The Kiln.

How it works

Manganese can hold different amounts of oxygen, and each form has its own colour:

Form Colour Where you see it
Manganese dioxide Black-brown The ore (pyrolusite); the brown stain left after permanganate works
Potassium manganate Dark green The melt after fusing ore with potash
Potassium permanganate Deep purple The finished product

Step 1 — fusion. Black manganese dioxide heated with caustic potash and an oxidiser — oxygen from the air, or saltpeter — becomes green potassium manganate. It is stable only in strong alkali.

Step 2 — conversion. Make the green solution less alkaline — most simply by bubbling carbon dioxide through it — and manganate splits itself: two-thirds becomes purple permanganate, one-third falls back to brown manganese dioxide (which you save and fuse again). Old chemists called the green melt "mineral chameleon", because its solution turns from green through blue and violet to purple as you watch.

Step 3 — crystals. Permanganate dissolves moderately in cold water (about 6 g in 100 ml at 20 °C) and four times better in hot (about 25 g at 65 °C). So a hot strong solution, cooled, gives dark needles.

Why it disinfects and cleans. Permanganate is an oxidiser: it tears electrons from other substances — germs, smelly sulfur compounds, dissolved iron, the dyes in stains — and is itself reduced to harmless brown manganese dioxide. That is why it stains skin brown and why its colour disappears when it works.

What you need

Item Amount Notes
Manganese ore, finely ground 100 g Pyrolusite; see below
Caustic potash (potassium hydroxide) 130 g for saltpeter route; 200 g for air route Lye and Potash — dry, solid sticks or lumps
Saltpeter (potassium nitrate) 120 g (saltpeter route only) Saltpeter
Iron pot or crucible, 1 litre Caustic melts eat clay and glass
Iron stirring rod
Source of carbon dioxide Chalk or limestone + dilute acid, or a jar of fermenting mash Hydrogen, Oxygen and Gases, Fermentation
Glazed crock or glass jar 3 litres For converting and settling
Glass wool or a bed of clean washed sand in a funnel Permanganate eats paper and cloth
Porcelain or glazed evaporating dish
Glass eye protection, leather gloves Molten caustic spits

Where to find it

Manganese ore is common worldwide (Finding and Identifying Ores, Rocks and Minerals):

  • Pyrolusite — black to steel-grey, soft, sooty; it blackens fingers and paper, with a black streak. Often in radiating needles or crusts.
  • Psilomelane — harder, black, in smooth rounded lumps like bunches of grapes, with a brownish-black streak.
  • Wad and bog manganese — soft black earthy masses in bogs, lake beds and old iron-ore beds, often mixed with bog iron (Iron (the Bloomery)).
  • Dendrites — black fern-like patterns on cracks in rock show manganese is nearby, but they are too thin to collect.

Tests: heavier than charcoal (about 4–5 times water); not attracted by a magnet. Melt a pinch with a little borax on a loop of wire in a flame (Identifying Substances): the glass bead turns amethyst violet. Best of all, melt a pinch with lye and a crystal of saltpeter on a scrap of iron: a green melt that turns pink-purple in water proves manganese — and is this whole chapter in miniature.

Caustic potash comes from wood ash, by way of potash and slaked lime (Lye and Potash). Caustic soda (from soda ash) also works, but gives sodium permanganate, which is so soluble that it will not crystallise easily — you get a strong purple solution (the old Condy's fluid) instead of crystals. That is still useful.

Step by step

1. Fuse 2. Dissolve 3. Turn purple 4. Crystallise chalk + acid ground ore + causticpotash (+ saltpeter),iron pot; melt turns green cold water: dark greenmanganate solution;ore residue settles bubble carbon dioxide untila drop is purple with nogreen edge; brown sludge falls filter through sand orglass wool; boil down,cool: dark needles brown sludge and residue go back into the next fusion
Fig. 1 Making permanganate. Ore and caustic potash are fused to a green manganate cake, dissolved, and turned purple by bubbling carbon dioxide through; the brown sludge is saved for the next batch, and the clear purple liquid is evaporated and cooled to dark crystals.

1. Grind and dry

Grind the ore as fine as flour in a stone mortar and sieve it through cloth. Dry it on a hot iron plate. Fine grinding matters more than anything else: coarse grains stay black in the middle.

2a. Fusion with saltpeter (faster)

  1. Melt the 130 g caustic potash in the iron pot over a charcoal fire. It melts at about 400 °C, just below a visible red glow, into an oily liquid. Wear eye protection from now on — a drop of molten caustic in the eye blinds.
  2. Stir in the 120 g saltpeter until it dissolves.
  3. Add the 100 g ground ore a spoonful at a time, stirring. It froths and spits; wait for each spoonful to settle.
  4. Raise the heat to a dull red and keep stirring for 20–30 minutes, until the mass thickens into a dark, almost black paste. A crumb dropped into water turns it deep green.
  5. Tip the paste out onto an iron plate to cool, then break it up. Keep it in a closed jar; damp air spoils it.

2b. Fusion in air (slower; needs no saltpeter)

  1. Dissolve 200 g caustic potash in as little water as possible, and stir in the 100 g ore to a thick paste.
  2. Spread it 1–2 cm deep in an iron pan and dry it over a gentle fire.
  3. Roast it at a heat that browns a scrap of paper laid on it within a minute but does not set it alight — about 250–350 °C — for 4–6 hours, breaking up lumps and turning the mass every 15 minutes so air reaches every grain. It turns from black to a dark green-black crumble. A kiln-heated iron tray in a The Kiln flue does well for larger batches.

The air route is how factories did it for a century; it makes no by-products that waste your permanganate later.

3. Dissolve the green cake

Crush the cake and stir it into 1 litre of cold water. Most dissolves to a dark green liquid. Let the black undissolved ore settle and pour the green liquid into the converting jar. Save the black residue for the next fusion.

4. Convert to purple

  1. Make carbon dioxide: drip dilute Hydrochloric Acid or vinegar onto lumps of chalk or limestone in a corked bottle and lead the gas through a tube to the bottom of the jar (Hydrogen, Oxygen and Gases). The gas from a vat of fermenting beer mash works too, piped from under a lid.
  2. Bubble it slowly through the green liquid. The colour moves through blue-green and violet to purple, and a brown cloud of manganese dioxide forms.
  3. Test often. Dip a glass rod and touch it to a white plate: you want a pure purple-red spot with no green edge. Then stop — too much carbon dioxide does no harm but wastes time.
  4. Let the brown sludge settle overnight. Siphon or pour off the clear purple liquid.

Without carbon dioxide you can do it with a little dilute Sulfuric Acid, added a few drops at a time with stirring until the green is just gone, or simply by boiling the green solution with plenty of water for an hour — slower and less complete.

5. Filter and crystallise

  1. Filter the purple liquid through a plug of glass wool or a bed of clean washed sand in a funnel. Not paper or cloth — permanganate eats them and is lost.
  2. Evaporate in a glazed dish until it is about a third of its volume, or until a drop on a cold plate shows crystals at its edge.
  3. Cover and cool slowly overnight. Dark purple, almost black needles with a greenish-bronze sheen grow on the bottom.
  4. Pour off the liquor and evaporate it again for a second crop.
  5. For purer crystals, dissolve them in the least possible hot distilled water (about 4 ml per gram at 65 °C), and cool again.
  6. Dry on a glass plate somewhere warm — not above about 100 °C, as permanganate breaks down at higher heat.

Yield: from 100 g of good ore expect 40–70 g of crystals, plus brown sludge to refuse. Mix the sludge back into the next fusion.

Store in a stoppered glass jar, away from anything that burns.

Using it

Strengths

The easiest way to measure is to make a stock solution and dilute it.

Stock (1 %): 1 g of crystals — about a quarter of a level teaspoon — fully dissolved in 100 ml of water. It is deep purple-black and too strong for skin. Keep it in a dark stoppered bottle.

Crystalsburn skin;always dissolvecompletely 1 ml stockin 100 ml water 1 ml stock in 2–10 litres of water 1 % stock1 g in 100 mldeep purple-blacknever on skin 0.01 % (1 in 10,000)pale rose pinkmake fresh each timeskin soak, 10–15 minutes 1–5 mg per litrebarely tinted,fades in minuteswell water: iron, smell Hold each glass against white paper in daylight to judge the colour
Fig. 2 Strengths by colour. Dilute the 1 % stock to the colour shown. Undissolved crystals and the stock itself burn skin; a soak should be the pale pink of a rose petal, and water treatment barely tints the water.
Use Strength How to make Looks
Titration standard 0.316 % (3.16 g per litre) Weighed exactly Deep purple
Skin soak 0.01 % (1 in 10,000) 1 ml stock in 100 ml water, or 10 ml in a litre Pale pink
Water: iron and smell 1–5 mg per litre About 1 ml stock per 2–10 litres Faint pink that fades
Pollution test A drop of 0.01 % in a glass of the water — —

Skin soaks

For weeping eczema, oozing or blistering skin, infected or fungal feet, and dirty leg ulcers:

  1. Make a 0.01 % solution fresh, with warm boiled water. Stir until no crystals at all remain — a single undissolved crystal burns a hole in skin.
  2. Soak the area for 10–15 minutes, once or twice a day, for a few days, until the weeping stops. Then pat dry.
  3. Protect the nails with a smear of fat; they stain brown for weeks.
  4. Never use it on the face, near the eyes, inside the mouth, the vagina or any body opening, or on large raw areas. Stop if the skin becomes sore or dry.

It is not a cure for deep infection, fever or spreading redness — those need Wound Care and Antiseptics, and if available Sulfa Drugs or Penicillin.

Water

  • Iron, manganese and rotten-egg smell. Add permanganate until a very faint pink just lasts 15 minutes, let the brown and rusty particles settle, then pass the water through a sand filter (Water Treatment for a Town). The pink must be gone before drinking.
  • It is not a reliable disinfectant for drinking water. In the 1890s wells in India were "pinked" during cholera epidemics, but chlorine kills germs far more surely at doses that are safe to drink. Use Chlorine and Bleach or boiling for that.

The pink test for pollution

Fill two clean glasses: one with water you know is good (rainwater, boiled), one with the water to test. Add the same drop of 0.01 % permanganate to each and set them side by side in shade. Clean water stays pink for hours. Water carrying sewage, manure or rotting plants turns yellow-brown in minutes. It is not proof that water is safe — germs can be present in clear water — but it shows which source is worse (Sanitation and Germs).

Titration

Permanganate needs no indicator: the purple disappears while there is anything left for it to oxidise, and the first drop of excess turns the whole liquid faint pink.

  • Standard: 3.16 g of pure crystals in 1 litre of distilled water. Let it stand a week in the dark and filter through glass wool; then check it against pure, bright iron wire: 0.100 g of iron dissolved in dilute sulfuric acid (with air kept out under a loose stopper) should take about 17.9 ml.
  • Iron in an ore: dissolve the weighed ore in dilute sulfuric acid (not hydrochloric, which the permanganate also attacks), reduce it fully to the pale green form with a little zinc, and titrate. Each ml of standard = 5.6 mg iron (Finding and Identifying Ores).
  • Organic matter in water ("oxygen demand"): to 100 ml of sample add 5 ml of dilute sulfuric acid and exactly 10 ml of the standard diluted ten times, and boil 10 minutes. If the pink has gone, the water is heavily polluted; how much extra it takes to keep it pink measures how much.

Other uses

  • Wood stain: a 2–5 % solution brushed on pale wood gives brown shades within minutes as it reacts with the wood. Rinse after.
  • Fruit storage: soak small pieces of fired clay in a strong solution, dry them, and put a handful in a cloth bag among apples or bananas; replace when they turn brown (Preserving Food, Granaries and Food Storage).
  • Removing stains: brown permanganate stains come off skin and cloth with lemon juice, vinegar with a pinch of wood-sorrel salt, or a weak solution of sulfite from Photography.

How to tell it worked

  • Crystals: dark purple to black needles with a bronze-green shine; a single crystal dropped into a glass of water sends down purple streamers.
  • Strength: 1 g colours 10 litres clearly pink.
  • Activity: add a few drops of solution to a little green vitriol (Sulfuric Acid) solution with a drop of acid — the purple vanishes instantly. Hydrogen peroxide or oxalic acid from wood sorrel (Oxalic Acid) does the same, with fizzing.
  • Purity: the crystals should dissolve completely in hot water. A green tint means manganate is left — dissolve and treat with carbon dioxide again.

Note Troubleshooting. Cake gives little green colour → ore ground too coarsely, not enough heat or time, or too little potash; or the ore was not manganese — test it. Grind finer and roast longer with more stirring. Green solution stays green with carbon dioxide → too alkaline: dilute it with twice the water and continue. Purple solution turns brown overnight → paper, cloth, dust or organic matter got in; or it was heated too long. Filter through glass wool and keep covered. No crystals on cooling → too dilute; boil down further. If you used caustic soda, it will not crystallise — keep it as solution. Crystals are brown and crusty → dried too hot. Redissolve and recrystallise.

Dangers

Danger Molten caustic potash blinds and burns to the bone. It spits when ore or water is added. Wear glass eye protection, gloves and long sleeves; keep a bucket of clean water at hand to wash splashes for 20 minutes or more (Lye and Potash, Emergencies). Never let water fall into a pot of molten caustic.

Danger Permanganate starts fires and explosions with the wrong partners. Mixed with glycerine, sugar, sawdust, sulfur or charcoal powder, it can burst into flame on its own. With concentrated sulfuric acid it forms a red-green oil that explodes violently. Store it alone, in glass, away from fuels and acids; never grind it with anything; keep every scrap of fuel and organic matter out of the saltpeter fusion. Clean up spills with plenty of water, not with sawdust or rags.

  • Crystals burn skin and eyes. Always dissolve completely before any use on the body; handle crystals with a spoon, not fingers.
  • Poison. Swallowed, crystals or strong solutions burn the mouth, throat and stomach, and as little as 10 g can kill an adult. People have died from swallowing it in despair; keep it locked away (Mental Health and Trauma). If swallowed, rinse the mouth and give small sips of water or milk; do not make the person vomit; get help (Emergencies).
  • Manganese dust. Years of breathing manganese ore or oxide dust damages the nervous system, with shaking and stiffness like old age. Grind ore wet or under a cloth, and outdoors.
  • Carbon dioxide pools in low places; convert in a ventilated room, not a cellar.

What this unlocks

Permanganate is a standby for skin and wound care in any clinic (The First Aid Kit, Nursing the Sick), a tool for cleaning iron-laden well water, and the first self-indicating titration reagent in Identifying Substances, used for iron in Finding and Identifying Ores and organic pollution in Water Treatment for a Town. The same green manganate fusion is the oldest test for manganese, and permanganate is used in the laboratory to make oxygen and chlorine in small amounts (Chlorine and Bleach) and to oxidise other chemicals.

How it was first done

In 1659 the German chemist Johann Rudolf Glauber fused pyrolusite with potash and saltpeter and noticed that the melt, dissolved in water, changed from green to purple. Through the 1700s it was a curiosity called mineral chameleon; Carl Wilhelm Scheele studied it in 1774, in the same work in which he discovered chlorine and noted the existence of manganese. In the 1850s the London chemist Henry Bollmann Condy patented solutions of sodium and potassium permanganate as disinfectants — Condy's fluid and Condy's crystals — sold for cleaning wounds, rooms and drinking water. The volumetric use of permanganate to measure iron was introduced by Frédéric Margueritte in 1846, and it became one of the standard methods of nineteenth-century chemical analysis.

Source: content/entries/chemistry/permanganate.md