◆ Rebuild

Part 5 · Cloth and Clothing

Tablet and Band Weaving

Narrow woven bands — straps, belts, tapes, harness and trim — made on a small inkle loom or by turning a pack of square cards with holes in their corners. Bands are the strongest thing you can weave for their size, need almost no equipment, and are the quickest way to learn weaving.

Difficulty
●●●●●
Time
A day to make an inkle loom or a set of cards; a metre of band takes 2–4 hours
Steps from zero
2 prerequisites →

You need first

Spinning and Weaving Cloth

This unlocks

Elastic and Rubber Thread
The full path from nothing — 2 steps before this one
  1. Cordage and Rope
  2. Spinning and Weaving Cloth
  3. Tablet and Band Weaving

Do them roughly in this order. See it on the tech tree →

Why it matters

A great deal of what holds a household together is not cloth but band: narrow, strong strips a few centimetres wide. Belts and braces. Straps for carrying baskets, firewood and babies (Nappies, Feeding Bottles and Baby Gear). Ties for bags, aprons and bed curtains. Tape to bind the raw edges of clothes (Sewing, Needles and Thread, Making Clothes) and roll up bandages (Wound Care and Antiseptics). Garters to hold up stockings (Knitting, Crochet and Netting). Head straps (tumplines) that let a person carry 30 kg on their back. Halters, girths and traces for horses and oxen (Draft Animals and Harness, Bits, Stirrups and Spurs, Riding and Training Horses). Laces for shoes (Footwear). Guitar and drum straps (Musical Instruments). Decorative borders sewn on clothes.

Leather does many of these jobs, but leather needs a dead animal and weeks of tanning (Hides and Leather). A woven band needs only yarn and a few sticks, it does not stiffen or rot when wet the way rawhide does, and it can be made to any length.

Band weaving is also the best way to learn weaving. A band is narrow, so every mistake is visible and quick to fix, and a beginner finishes something useful in an afternoon. Everything you learn here — warp, weft, shed, beating, keeping an even edge — carries straight over to the broad The Loom.

How it works

Ordinary cloth is balanced: the warp (lengthwise threads) and weft (crosswise threads) are equally spaced and both show. A band is usually warp-faced: the warp threads are packed so tightly side by side that they completely hide the weft. Only the warp shows, so the colour order of the warp makes the pattern, and the weft becomes an invisible thread that simply locks the warp together.

This has two big advantages. First, all the strength lies along the length, where a strap needs it: a band of 40 warp threads has 40 threads pulling together. Second, the weft, pulled snug at every pass, draws the band in to a firm, even width and makes it stiff and hard-wearing.

There are two ways to open the shed (the gap between raised and lowered warp threads through which the weft passes):

  • Heddles. As on any loom (Spinning and Weaving Cloth), every other thread is held in a string loop at a fixed height; the threads between are free and can be pushed up or down by hand. This is the inkle loom, and also the small slotted band heddle used with a backstrap.
  • Tablets. Each group of four warp threads passes through the four corner holes of a square card. Two threads are on top and two below, so there is a shed between them. Turn the card a quarter turn and a different pair comes to the top: a new shed. Because the four threads of each card twist round each other as you turn, each card makes a tiny four-strand cord, and the weft binds the cords side by side. Tablet bands are thick, extremely firm and almost do not stretch — the best weave there is for straps that carry weight.

What you need

Item Size Notes
Yarn 100–300 g for a 2 m belt Smooth, strongly twisted, plied yarn: worsted wool (Wool), linen or hemp (Flax, Hemp and Linen). About 1–2 mm thick. Fuzzy, soft yarn sticks to itself and will not open a clean shed
Weft A third as much as warp The same yarn, or thinner, in the edge colour
Inkle loom Base 80–90 cm Hardwood; see Method 1
Heddle thread 5–10 m Strong, smooth linen or hemp thread
Tablets 20–30 cards, 6–7 cm square Thin wood, rawhide (Hides and Leather), bone or horn (Horn and Bone Working), 1–2 mm thick
Shuttle / beater 25 × 4 × 0.6 cm A flat hardwood stick, one edge planed thin like a blunt knife. You wind weft on it and beat with its edge
Backstrap 50 × 8 cm A strip of leather or thick cloth with a cord at each end, for tablet weaving
Tools Knife, saw, an awl or bow drill for holes (Drills and Boring), sandstone to smooth edges

Where to find it

  • Yarn. Spin it yourself on a drop spindle (Spinning and Weaving Cloth) or The Spinning Wheel, from long-stapled wool combed rather than carded (combed "worsted" yarn is smooth and strong), or from line flax or hemp. Spin firmly and ply two singles together. A good test: hold 30 cm of yarn between your hands and pull hard. It should not drift apart, and when you let go, it should not kink up into a tangle (if it does, the twist is unbalanced — wash and dry it under light tension).
  • Wood for the loom. Any straight-grained, well-seasoned hardwood (Basic Woodworking): oak, ash, beech, maple, birch, fruit woods. Pegs of the same, or of straight hazel or ash rods 2–2.5 cm thick, dried and peeled.
  • Card material. Thin boards split and shaved from straight-grained wood such as lime (basswood), birch or poplar; rawhide scraped thin and dried flat under a weight; the flattened shoulder blades of sheep; flat horn plates (see Horn and Bone Working). The surface must be smooth so the yarn slides.

Method 1: The inkle loom

The inkle loom holds a continuous loop of warp stretched round a set of pegs, so a band about 2 metres long fits on a frame less than a metre long. Every other thread passes through a fixed string heddle; the threads between are open.

Front peg Woven bandtravels roundthe pegs Shedthe weft passes here Top pegopen threads ride over it Open threadsdashed; free to move Heddled threadsheld level by loops Heddle loopson the heddle peg,all the same length Tension pegwedge locks it Back pegs THE TWO SHEDS, LOOKING ALONG THE WARP Shed 1push open threads down Shed 2lift open threads up weft
Fig. 1 An inkle loom from the side. The warp runs round the pegs in a continuous loop. Heddled threads (solid) are held at one level by string loops tied round the heddle peg; open threads (dashed) ride over the top peg, so a shed opens in front. The finished band moves round the loop as you weave.

Build it

  1. Base: a beam 85 × 7 × 4 cm.
  2. Uprights: three posts 7 × 4 cm — a front post 35 cm tall at one end, a back post 40 cm tall at the other, and a heddle post 40 cm tall about a third of the way from the front. Fix each into the base with a through mortise and a wedged tenon so it cannot rock (Basic Woodworking, Doors, Windows and Joinery).
  3. Pegs: 2.5 cm round rods, 15–18 cm long, driven tightly into 2.5 cm holes so they stick out to one side. You need: one front peg at the top of the front post; one lower front peg 20 cm below it; a top peg at the top of the heddle post; a heddle peg 12 cm below the top peg on the same post; two back pegs on the back post, top and 20 cm lower.
  4. Tension peg: cut a slot 2.5 cm wide and 12 cm long along the base between the heddle post and the back post. A peg set in a small block slides along the slot and is locked with a wedge driven beside it. Sliding it lets you tighten the warp, and loosen it as weaving takes up length.
  5. Smooth everything with a scraper, sandstone and a rub of beeswax or fat, so the warp glides round the pegs.

Make the heddles

All heddles must be the same length, or the shed will be ragged.

  1. Drive two smooth pegs into a board, spaced so that a loop round them, when hung from the heddle peg, reaches just up to the line of the warp from the front peg to the top back peg — usually 11–13 cm apart. Hang one test loop first and check it.
  2. Wind strong linen thread once round both pegs and tie it with a square knot (Cordage and Rope) tight against one peg. Slip it off. Repeat. You need half as many heddles as warp threads, plus a few spare.

Warp it

  1. Plan the band on paper. Write the colour of each thread in order, marking each one H (heddled) or O (open), alternating H, O, H, O... For a first band: 41 threads, with the two edge threads of each side the same colour.
  2. Tie the yarn to the tension peg. For an H thread, take it from the tension peg round the lower front peg, up over the front peg, through a heddle loop (hang the loop on the heddle peg, pass the thread through it), over the top back peg, down round the lower back peg and back to the tension peg. For an O thread, take the same path but pass it over the top peg instead of through a heddle.
  3. Keep the same, firm tension on every thread — snug, not banjo-tight. When you change colour, tie the old and new yarn together at the tension peg.
  4. Push all the threads together into a neat bundle on each peg.

Weave

  1. Wind the weft onto the flat shuttle: 3–5 m at a time, wound in a figure-of-eight along its length.
  2. Open the first shed. Stand or sit at the front. Push the open threads down with your flat hand just behind the heddles. The heddled threads now lie on top: there is a shed between the two layers in front of the heddles.
  3. Pass the weft through the shed, leaving a 10 cm tail. Beat it back towards the front peg with the edge of the shuttle.
  4. Change the shed. Lift the open threads up with your hand. Now they lie above the heddled ones. Beat again — beating into the new shed packs the last weft tight. Pass the weft back.
  5. Pull the weft snug. This is the whole art of a good band: draw the weft so that the edge threads just touch and no loop of weft shows at the edge, but not so hard that the band narrows. Make a width gauge — a stick with a notch cut exactly as wide as the band should be — and check every 5 cm.
  6. Repeat: down, weft, beat; up, beat, weft. Tuck the starting tail into the second shed.
  7. Advance the band. When you have woven to within 10 cm of the heddles, loosen the tension wedge, pull the whole warp loop round the pegs so the woven part moves round towards the bottom, and tighten again.
  8. Finish when the unwoven warp is too short to open a shed, usually after 1.6–2 m of band. Cut the warp at the unwoven section. Tie the ends in groups of four with overhand knots, or braid them, or fold the end over twice and hem it (Sewing, Needles and Thread).

Width. With yarn about 1.5–2 mm thick, a warp-faced band packs 10–14 threads per centimetre: 41 threads make a band about 3–4 cm wide.

Patterns from the warp

Because only the warp shows, and the heddled and open threads take turns on top, the colour plan gives you patterns without any extra work:

  • H and O both colour A, then both colour B, in blocks → lengthwise stripes.
  • All H threads colour A and all O threads colour B → crosswise bars across the band, A and B alternating at every pass.
  • A single H thread of A among B → a line of dots.

Pick-up patterns: warp a band with all H dark and all O light (or the reverse). Then, in each shed, use a pointed stick to lift chosen threads from the lower layer to the top before passing the weft. Each thread lifted makes a "float" of colour; with planning you can weave letters, diamonds and crosses. Work them out on squared paper first.

Method 2: Tablet (card) weaving

Tablet weaving needs no loom at all: a set of cards, a post or door frame to tie to, and your body to give tension.

ONE CARD S AND Z, FROM ABOVE THE SHED, FROM THE SIDE ABCD Quarter turnbrings a new pair of holesto the top: a new shed Sleans / Zleans \ S and Z cords lean oppositeways; mixing them makes a V Shedweft goes here band Backstraplean back to tension Woven bandrolled onto a stick Card packall turned together Twist builds upreverse to undo it Warp4 threads per card, 2–3 m Postor door frame
Fig. 2 Tablet weaving. Each card carries four threads through its corner holes; turning the whole pack a quarter turn brings a new pair of threads to the top and opens a new shed. Threads entering from one face (S) or the other (Z) make the cords lean opposite ways. One end of the warp is tied to a post, the other to a strap round the weaver's waist.

Make the cards

  1. Cut 24 squares 6–7 cm across from thin wood, rawhide, bone or horn, 1–2 mm thick. All exactly the same size: cut one perfect card, then draw round it for the rest.
  2. Round the corners slightly.
  3. Make a hole 5–6 mm across about 1 cm in from each corner. Smooth the inside of each hole with a twist of sandpaper made from sand glued to cord, or by working a round stick with fine sand back and forth through it. A rough hole frays the warp.
  4. Mark the holes A, B, C, D clockwise on one face of every card, and number the cards 1 to 24.

Thread them

  1. Cut the warp. For a 1.5 m band, cut threads 2.2 m long — four per card, 96 threads for 24 cards. Warp loss at each end is about 30–40 cm.
  2. Choose the direction. Hold a card upright, its marked face to your left. Each thread can pass through its hole from the marked face to the back (call it S) or from the back to the marked face (Z). Thread all four holes of one card the same way. Looked at from above, an S card leans one way and a Z card the other.
  3. For a first band: thread cards 1–12 S and 13–24 Z. Put a dark thread in holes A and B and a light thread in C and D of every card, except two cards at each edge, which get four threads of the edge colour.
  4. Tie the far ends of all threads together in one firm knot and tie it to a post, a door handle or a heavy chest. Stand back, comb the threads straight with your fingers so each has the same tension, and tie the near ends together. Tie the near knot to your backstrap.
  5. Stack the cards into a tight pack, standing on edge, faces parallel to the warp, all with the A hole in the same position (top far corner).

Weave

  1. Sit back until the warp is firm. The cards hang in the middle of the warp, and between the two top threads and the two bottom threads of each card there is a shed.
  2. Pass the weft through the shed close to you. Leave a tail.
  3. Turn the pack a quarter turn away from you (forward), all cards together. Hold the pack edge-on between your hands and roll it. A new pair of holes comes to the top, and the shed changes.
  4. Beat the new shed towards you with the shuttle edge, pushing the crossing of the threads tight against the last weft.
  5. Pass the weft back. Pull it snug so the edges are straight and the width constant.
  6. Repeat: turn, beat, weft. Slide the pack along the warp away from you every few centimetres to keep a good shed.
  7. Roll up the band as it grows: untie the near knot, wrap the band round a stick, and tie the stick to your backstrap.

Twist builds up

Each forward turn twists the four threads of every card round each other — in front of the cards, where they become the band, and also behind them, where they wind up into a hard twist. After 20–30 turns forward the warp behind the cards is so twisted the shed will barely open.

The answer is to turn backwards for a while. Turn back the same number of times you turned forward; the twist behind unwinds, and the cords in the band lean the other way, which makes a zigzag. Many weavers simply turn 4 forward, 4 back, or 8 forward, 8 back, and use the zigzag as the pattern. Alternatively, untie the far end every metre and let the twist shake out.

Tip Reading a pattern. Write the threading as a grid: four rows (holes A to D) and one column for each card, colouring each square, with S or Z under each column. Every quarter turn shows the colours of the next row on top. With the A-B dark, C-D light threading above, forward turning gives diagonal lines meeting in a V down the middle; changing direction every 4 turns turns them into diamonds.

Width and strength. Each card adds a little more than the thickness of one yarn to the width: 24 cards with yarn about 1 mm thick make a band about 2.5–3 cm wide and 3–4 mm thick. Woven in linen or hemp, such a band holds the weight of a person.

Method 3: The band heddle

Across Scandinavia and the Baltic, bands were woven with a band heddle: a small rigid heddle 15–20 cm wide, a row of thin wooden slats each with a hole in its middle. Warp threads pass alternately through holes and slots; lifting and lowering the heddle makes the two sheds, as on the frame loom (The Loom). Tie the warp between a post and your backstrap and weave as with tablets.

How to tell it worked

  • Even width. The band matches the width gauge along its whole length, within 1–2 mm. Edges are straight, without loops of weft or pinched "waists".
  • Warp-faced. No weft shows on the face except, at most, a tiny dot at each edge.
  • Firm. Pinched between finger and thumb, the band feels like a strap, not like cloth. A tablet band should hardly bend sideways at all.
  • Strength. Hang a bucket of water or stones from a 30 cm piece and add weight. A strap you will trust with a load should hold five times that load without stretching or breaking.

Note Troubleshooting. Band narrows and widens → you are pulling the weft unevenly; use the width gauge, and pull each weft until the edges just touch. Weft shows through → warp too thin or too widely spaced; use more threads, thicker yarn, or beat harder. Shed won't open on the inkle → heddles of different lengths, or the warp is too slack; remake the long ones and tighten the tension peg. Sticky, hairy yarn also clings: use smooth worsted or linen. Tablet threads tangle behind the cards → twist build-up; reverse the turning direction or shake the twist out. A card flips over or turns alone → it was threaded the wrong way or slipped out of the pack; check that all A holes are in the same position before every turn. Loops at one edge on tablet bands → the edge cards need four threads of the same colour, turned always the same way as their neighbours, and the weft pulled firmly.

Dangers

Band weaving is one of the safest crafts in this book, but:

  • Posture. Hours bent over a backstrap or a low inkle loom hurt the back and neck. Sit upright with the work at chest height, and stop to stretch every half hour.
  • Cords and children. Long warps, loose cords and straps tied to posts are strangling hazards for small children. Never leave a child alone with them, and never put a cord round a baby's neck.

Warning Trusting a strap. A strap that carries a load — a baby sling, a tumpline, a horse's girth or a lifting strap — must be woven from strong linen or hemp, tested to five times its working load, and inspected often. Bands wear thin where they rub over buckles and edges; replace them before they fray through, not after.

What this unlocks

With bands you have belts, straps and harness without leather (Draft Animals and Harness, Wagons and Carriages); tape for binding seams and bandages (Sewing, Needles and Thread, Wound Care and Antiseptics); starting borders for the warp-weighted loom (Spinning and Weaving Cloth); and decorative trim for Making Clothes. Toggles, buckles and rings to fasten them come from Horn and Bone Working and Blacksmithing. The four-strand twist of tablet weaving is close kin to rope (Ropewalks and Sailcloth) and braid (Cordage and Rope). The same principle — many small units, each lifted or turned separately to make a pattern — is the idea behind the Jacquard loom (Textile Machinery).

How it was first done

Narrow bands were probably among the very first things ever woven, since a short warp held between a branch and a person's waist needs no loom at all. Tablet weaving is old: bands with the distinctive four-strand twist survive from the Early Iron Age salt mines of Hallstatt in Austria (about 800–400 BC) and from princely graves of the same period in central Europe. The most famous find is the Oseberg ship burial in Norway (AD 834), which held a tablet-woven band still in progress on a set of 52 wooden tablets. Band heddles were used in Scandinavia and the Baltic into modern times, and backstrap band weaving lives on in the Andes and Asia. In 16th-century England, inkle was the word for narrow linen tape sold by pedlars; the inkle loom that bears its name is a simple folk tool that became widely popular again with hand weavers in the 20th century.

Source: content/entries/textiles/band-weaving.md