◆ Rebuild

Part 15 · Knowledge and Science

Vacuum Coating and Thin Films

In a good enough vacuum, a metal boiled off a hot tungsten wire flies in straight lines and lands as a film a ten-thousandth of a millimetre thick on everything it faces. That is how telescope mirrors are aluminised, lenses given purple anti-reflection coats, laser mirrors made 99.9 % reflective from clear materials, and chips and plastic film metallised. How to build the coater and its diffusion pump, aluminise a mirror, coat a lens, stack a dielectric mirror, and sputter metals that will not evaporate.

Difficulty
●●●●●
Time
Weeks to build a coater and diffusion pump; an afternoon per coating run
Steps from zero
31 prerequisites →

You need first

The Vacuum PumpMirrorsLenses

This unlocks

High-Vacuum Pumps and Gauges
The full path from nothing — 31 steps before this one
  1. Fire
  2. Stone Tools
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Basic Woodworking
  8. Hunting and Trapping
  9. The Kiln
  10. Pottery
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Mercury
  15. Lye and Potash
  16. The Wheel and Axle
  17. Glass
  18. Bellows
  19. Saltpeter
  20. The Lathe
  21. Copper Smelting
  22. Lead
  23. Laboratory Glassware
  24. Sulfuric Acid
  25. Pumps
  26. Lenses
  27. Gold and Silver
  28. Nitric Acid
  29. The Vacuum Pump
  30. Silver Nitrate and Silver Salts
  31. Mirrors
  32. Vacuum Coating and Thin Films

Do them roughly in this order. See it on the tech tree →

Why it matters

A telescope mirror silvered with chemicals (Mirrors) tarnishes yellow within months and must be stripped and redone. An aluminised mirror, coated in vacuum, reflects nearly as well, reflects ultraviolet that silver does not, and stays good for years. Every large telescope since the 1930s has been aluminised (The Telescope, Building an Observatory).

The same machine does much more:

  • An uncoated lens surface throws back about 4 % of the light. A binocular or camera lens has 6 to 16 such surfaces, losing a third or more of the light and filling the picture with glare. One coat of a clear fluoride, a quarter of a wavelength thick, cuts each loss to about 1 % (Lenses, Photography).
  • Stacks of clear layers make mirrors that reflect 99.9 % of one colour, which lasers need (Lasers), and filters that pass one colour only (The Spectroscope).
  • Metal films wire every chip (Integrated Circuits), make the shine on plastic reflectors and food wrappers (Sacks, Boxes, Crates and Packaging), and coat window glass to keep heat in.

How it works

Straight flight in a vacuum. Heat aluminium on a tungsten wire to about 1,200 °C and atoms boil off it. In air they hit gas molecules within a fraction of a millimetre and drift as smoke. Pump the air out until the pressure is about a ten-thousandth of a millimetre of mercury (0.013 pascals; ordinary air is 760 mm) and the average distance a molecule travels before hitting another (the mean free path) grows to about 50 cm. Now the atoms fly in straight lines, like light from a lamp, and condense as a smooth, shiny film on whatever cold surface they hit. Anything in their "shadow" stays bare.

How much metal. A small source sprays atoms equally in all directions. At distance r, the thickness laid down is the mass evaporated divided by the area of a sphere of radius r, divided by the metal's density. For aluminium (2.7 g per cm³) at 30 cm, 0.3 g makes a film about 100 nanometres thick (a nanometre is a millionth of a millimetre). Thickness falls with the square of distance: twice as far, a quarter as thick.

Interference. A clear film a fraction of a wavelength of light thick reflects light from both its top and bottom faces. If the film is exactly a quarter-wave thick (in the film, where light is slowed), the second reflection travels an extra half wave and arrives out of step with the first:

  • With a film whose refractive index is lower than the glass, the two weak reflections cancel: an anti-reflection coating.
  • With a film whose index is higher, they add. Stack alternating high and low quarter-wave layers, and the reflections from every boundary add up in step: a dielectric mirror, made only of clear materials, that reflects nearly all of one colour band and passes the rest.

Soap bubbles and oil films show the same effect (Forces, Energy and Heat).

Anti-reflection coating one low-index layer, a quarter-wave thick Dielectric mirror high and low layers, each a quarter-wave out of step: cancel in step: add up fluoride 100 nm glass almost all the light goes through grey = zinc sulfide (high), pale = fluoride (low)
Fig. 1 Thin films and light. Left, an anti-reflection coating: the reflections from the top and bottom of a quarter-wave low-index layer are half a wave out of step and cancel. Right, a dielectric mirror: alternating high- and low-index quarter-wave layers each reflect a little, all in step, adding to nearly all the light.

What you need

Item Notes
Bell jar and baseplate Thick glass jar 30–45 cm across, or a steel tank with a glass window; flat ground steel or brass plate (Laboratory Glassware, Machine Tools)
Rough pump Oil-sealed rotary pump reaching 0.01–0.05 mm of mercury
Diffusion pump Below; reaches 0.00001 mm with a cold trap
Gauges McLeod gauge and glow tube (The Vacuum Pump); a hot-wire (Pirani) gauge if you have one (High-Vacuum Pumps and Gauges)
High-current transformer 5–10 volts, 50–150 amps, with a control on the primary (The Transformer)
High-voltage supply 2–5 kV for glow cleaning and sputtering (The Induction Coil, Rectifiers: Turning AC into DC)
Sources Tungsten wire 0.5–1 mm; tungsten, molybdenum or tantalum sheet 0.1–0.2 mm for boats (Tungsten and Filament Wire)
Coating materials Purest Aluminium wire; magnesium fluoride; zinc sulfide; gold or silver (Gold and Silver)
Cooling Running water; ice and salt, or dry ice and alcohol, or liquid air for the trap (Liquid Air, Nitrogen and the Noble Gases)

Where to find it

  • Aluminium from bauxite (Aluminium). Impurities spoil the shine; use the purest you can make, as clean wire.
  • Magnesium fluoride: dissolve burnt magnesite (Firebrick and Refractories) in Hydrochloric Acid. Separately, fuse fluorite (purple-green fluorspar, Fluorspar and Fluorine Compounds) with an equal weight of soda ash and a little sand, and leach the cake with water: the liquid holds sodium fluoride. Mix the two solutions and fine white magnesium fluoride settles out. Wash it many times, dry it, bake it at 500 °C and press it into pellets.
  • Cryolite, a white glassy mineral from Greenland, is a natural low-index coating material that evaporates easily (Fluorspar and Fluorine Compounds).
  • Zinc sulfide: dissolve zinc (Zinc and Brass) in Sulfuric Acid, and add a solution of sodium sulfide (made by roasting Glauber's salt with charcoal). Pure white zinc sulfide settles out. Natural sphalerite is too impure.

The vacuum coater

Work, face down 25–60 cm above the sources aluminium film lands here Ring electrode for glow cleaning Shutter, swung open Tungsten filaments loaded with aluminium loops Copper rods 50–150 A at 5–10 V Bell jar on baseplate Cold trap ice and salt, dry ice or liquid air High-vacuum valve Rotary rough pump to about 0.01 mm roughing valve Diffusion pump vapour jets drive gas down; water- cooled walls heater and boiler transformer 2–5 kV A vacuum coater
Fig. 2 A vacuum coater in section. The work hangs face down at the top of the bell jar. Below it, behind a swinging shutter, tungsten filaments loaded with aluminium are fed by heavy copper rods from a low-voltage transformer. A ring electrode allows glow-discharge cleaning. The chamber is pumped through a cold trap by a diffusion pump, which is backed by a rotary pump.
  1. Chamber. For work up to 20 cm across, a heavy glass bell jar 30–45 cm across and 40–50 cm tall on a ground baseplate, sealed by a rubber gasket smeared thinly with vacuum grease (Packing, Gaskets and Seals). For bigger mirrors, a welded steel cylinder with a bolted lid and a glass window. Keep the inside spotless.
  2. Feedthroughs. Pass two copper rods 8–10 mm thick through the baseplate in glass or porcelain sleeves sealed with wax or rubber, to carry 50–150 amps to the sources. Add a high-voltage lead to an aluminium ring electrode for glow cleaning, and a shaft through a greased gland to swing a shutter.
  3. Sources. For aluminium, wind helical filaments: three strands of 0.5 mm tungsten wire twisted together, coiled into 6–8 turns, 1 cm across. Hang small loops of aluminium wire on each turn. For powders and pellets, fold a boat from tungsten or molybdenum sheet, 1 × 5 cm, with a dimple in the middle. Bolt sources between the rods.
  4. Work holder. A ring or plate at the top, holding the work face down, 25–60 cm above the sources. For lens coatings, add a heater behind the work: a coil of nichrome or a few lamps (Electric Kettles, Irons, Heaters and Cookers) to warm the glass to 250–300 °C.
  5. Pumping line. A wide tube, at least 5 cm, through a cold trap and a valve to the diffusion pump, with a second valve so the rough pump can pump the chamber directly first.

The diffusion pump

The piston, water-jet and mercury pumps of The Vacuum Pump are too slow or too weak for coating. A diffusion pump has no moving parts: a jet of hot vapour sweeps gas molecules downward to where a rough pump can take them.

  • Body: a vertical steel or copper tube 8–10 cm across and 35–45 cm tall, flanged at the top to the chamber valve. A copper water pipe is wound around it and soldered on along most of its length.
  • Boiler: the closed bottom, holding 50–100 ml of pump fluid, heated by a 300–600 watt electric heater underneath (Electric Kettles, Irons, Heaters and Cookers).
  • Jet stack: a central chimney with two or three umbrella-shaped caps stacked inside. Vapour rises up the chimney and shoots out from under each cap, downward and outward, at high speed toward the cold walls.
  • Foreline: a side pipe near the bottom, to the rough pump.

Gas molecules wandering into the top are struck by the vapour jet and driven down. The vapour hits the cold wall, condenses, and runs back to the boiler. A 10 cm pump moves a few hundred litres a second of thin gas. Sizing the backing pump, better gauges and finding leaks are covered in High-Vacuum Pumps and Gauges.

The fluid. Use mercury (Mercury), or a carefully chosen pump oil: the heaviest fraction of Petroleum and Refining distilled again under vacuum, so that it barely evaporates at room heat. Mercury vapour is poisonous and reaches the chamber unless a cold trap stops it.

The cold trap: a metal or glass U-bend or baffle between pump and chamber, cooled by ice and salt (−20 °C), dry ice in alcohol (−78 °C) or liquid air (−190 °C). It freezes out pump vapour and water.

Rules of use.

  1. Rough-pump the pump to below 0.1 mm before switching on the heater; the jet will not start against more.
  2. Water on before heat, always.
  3. Warm-up takes 15–30 minutes.
  4. Never let air into a hot oil pump: the oil oxidises and can catch fire. Close the high-vacuum valve, switch off, and let it cool 30 minutes before venting.

Step by step: aluminising a mirror

  1. Strip any old coating: silver in dilute Nitric Acid, aluminium in a weak solution of caustic soda (Lye and Potash). Rinse.
  2. Clean. Rub the face with a cream of precipitated chalk and water on cotton wool, rinse in clean water and then distilled water, and stand it on edge to drain. The breath test: breathe on it. Clean glass fogs evenly grey and clears evenly; greasy spots show as patterns. Clean again until it passes. Do not touch the face.
  3. Load. Fit fresh filaments and run them once, empty, red hot in vacuum to clean them. Hang the aluminium. Set the mirror face down above them. Several filaments in a ring under a large mirror give an even coat.
Mirror Throw (distance) Filaments Aluminium per filament
15 cm 30 cm 3 0.1 g
25 cm 45 cm 4–6 0.15 g
40 cm 60 cm 6–8 0.2 g
  1. Rough pump to about 0.05 mm.
  2. Glow clean. Switch the high voltage onto the ring for 5–10 minutes. A violet glow fills the jar and its ions scrub the glass. Switch off.
  3. High vacuum. Open the diffusion pump. Wait until the gauge reads 0.00005 mm (0.007 Pa) or better: typically 30–90 minutes. The glow tube shows no glow at all.
  4. Melt. Shutter closed, raise the filament current slowly until the aluminium melts and runs over the tungsten like solder, bright and wet. This takes 10–30 seconds and drives off gas.
  5. Flash. Open the shutter and turn the current up fast. The aluminium is gone in 2–5 seconds. Fast evaporation gives the brightest film. Close the shutter; switch off.
  6. Cool 15 minutes; close the valve; let air in slowly through a cotton-wool filter.

Protect it if you can: in the same run, evaporate a clear layer of magnesium fluoride, or of silicon monoxide (a mixture of fine silicon and quartz powder heated in a tantalum boat), about 150 nm thick. Bare aluminium grows its own thin oxide skin and lasts years; recoat when it dulls.

Good from bad. A good aluminised mirror is brilliant, faintly bluish-white, with no haze. Hold it up to a bright lamp: through a good coat the filament is barely visible, without bright patches or a sky of pinholes. Press sticky tape (Glues and Adhesives) on the edge and rip it off: the film stays. A milky, brown or grey film means poor vacuum, water vapour or slow evaporation. A film that peels means dirty glass.

Anti-reflection coatings

An anti-reflection coating is a single clear film a quarter-wave thick on each air–glass surface of a lens or window.

Magnesium fluoride is the usual material: refractive index 1.38, hard when laid on hot glass. On glass of index 1.52 it cuts the reflection of each surface from 4.3 % to about 1.3 % for green light. A lens of 4 surfaces passes 95 % instead of 84 %; a binocular with 10 surfaces, 88 % instead of 65 %. The quarter-wave for green light (550 nm) in magnesium fluoride is 100 nm.

  1. Clean the lenses as for a mirror, and set them face down in a holder, with a clean test glass beside them.
  2. Pump down. Heat the work to 250–300 °C behind a shutter. Cold-laid fluoride is soft and wipes off.
  3. Heat the boat of magnesium fluoride (it melts at 1,263 °C) until the pellets glow and start to evaporate. Open the shutter.
  4. Watch the colour of a white lamp reflected in the test glass through a window. As the film grows, the reflection dims and turns yellowish, then reddish-purple (green is being cancelled), then blue. Close the shutter when the reflection is deepest purple and dimmest.
  5. Cool slowly before letting air in, or the hot glass cracks.

Cryolite works the same way, with slightly better cancelling, but the film is soft and dislikes damp: use it only on inside surfaces. Coat both faces of every lens.

Good from bad. A coated lens looks deep purple or amber-purple in reflection and much darker than an uncoated one. Breathe on it: the fog should clear evenly. Rub it gently with a clean cloth: a good coating does not mark.

Dielectric mirrors

A dielectric mirror (multilayer mirror) is a stack of quarter-wave layers of a high-index material (zinc sulfide, index 2.35) and a low-index one (magnesium fluoride, 1.38), starting and ending with zinc sulfide.

Layers Reflects (at its design colour)
3 about 68 %
5 about 88 %
7 about 96 %
9 about 98.4 %
11 about 99.5 %
15 about 99.9 %

For red helium-neon laser light (633 nm), each zinc sulfide layer is 67 nm thick and each fluoride layer 115 nm. Zinc sulfide evaporates from a molybdenum boat at about 1,000 °C, coming off as a vapour without melting.

Thickness by eye is not enough here. Build an optical monitor: shine a beam of light of the design colour (a sodium lamp, a mercury lamp with a green filter, or the laser itself) through the test glass onto a photocell and meter (Photocells and Sensors, Measuring Electricity). As each layer grows, the reading falls (or rises) and turns back. Close the shutter exactly at each turning point: that is a quarter-wave. Later, a quartz crystal in the chamber does the same by mass: its frequency falls as the film lands on it.

A dielectric mirror reflects only a band about a third as wide as its colour's wavelength and passes the rest, so it looks coloured: a green mirror is pink-purple when you look through it. Uses: laser mirrors (Lasers), interference filters that pass one narrow colour, cold mirrors that reflect light but pass heat in projectors, and beam splitters.

Sputtering

supply −1 to −3 kV to the target Target disc of coating metal, 5–10 cm Glow in thin argon ions (red) strike the target; metal atoms (yellow) fall Work, coated Earthed plate 3–5 cm below the target to the pumps argon in, 3–13 Pa
Fig. 3 A simple sputter coater. Inside the jar, filled with thin argon, a disc of the coating metal forms the negative electrode at the top; the work rests on the earthed plate below. At 1–3 kilovolts a glow fills the gap; argon ions slam into the metal disc and knock atoms off it, and they settle on the work.

Some metals, such as platinum, tungsten and chromium, need too much heat to evaporate easily, and alloys evaporate unevenly. Sputtering knocks atoms off a cold metal plate instead.

A sputter coater is the same chamber with:

  • A target: a disc of the coating metal, 5–10 cm across, as the negative electrode at the top. Gold leaf on a copper disc does for gold.
  • The work on an earthed metal plate 3–5 cm below.
  • Gas: pump down hard, then let in argon (Liquid Air, Nitrogen and the Noble Gases) to about 0.02–0.1 mm (3–13 Pa). Air works for gold and platinum, which do not oxidise.
  • Power: 1–3 kilovolts direct current at 10–50 milliamps, from a rectified transformer with a series resistor to limit the current (Rectifiers: Turning AC into DC).

A violet glow fills the gap. Positive gas ions accelerate into the target and splash atoms out of it; they drift onto the work as a dense, tightly stuck film. It is slow, a few nanometres a minute, but even, and it coats round corners and odd shapes. Coating samples for an The Electron Microscope, and making electrodes on crystals and ceramics (Piezoelectric Crystals and Ceramics), are typical jobs. Industry puts magnets behind the target (a magnetron), which trap electrons near it and make sputtering ten times faster at a few hundred volts; with a little oxygen or nitrogen added it lays down oxides and nitrides, like the gold-coloured titanium nitride on drills (Titanium).

Coating chips and plastics

  • Chips: a micrometre of aluminium evaporated over the whole wafer, then etched into wires (Integrated Circuits, Making Microchips).
  • Plastic film: in a roll coater, a reel of film unwinds over a cooled drum above a row of hot boats fed continuously with aluminium wire, laying down 30–50 nm while the film runs at metres a second. The result is mirror film, emergency blankets, capacitor film (Resistors, Capacitors and Coils) and crisp packets (Petrochemicals and Modern Plastics).
  • Plastic parts (lamp reflectors, mirrors, trim): dry them well; paint a base lacquer to seal and smooth the surface, aluminise, then add a clear top lacquer.
  • Half-mirrors: a thin aluminium film, about 10–15 nm (stop when a lamp seen through it is as bright as its reflection), divides a beam for instruments (The Microscope).

How to tell it worked

  • The gauge reaches the target pressure in the same time every run; if it gets slower, look for a leak, a dirty jar or wet work.
  • Mirrors are bright and pinhole-free; coatings survive the tape test.
  • Coated lenses show even purple reflections across the whole face; the colour is the same at centre and edge.

Note Troubleshooting.

  • Will not pump below 0.001 mm → leak or wet chamber. Paint suspect joints with alcohol and watch the gauge jump; bake the jar gently; renew grease.
  • Diffusion pump does nothing → backing pressure too high, heater too weak, or no cooling water.
  • Milky or brown mirror → poor vacuum, slow evaporation, or impure aluminium.
  • Patchy, thin edge → sources too close or too few; move them farther away and spread them out.
  • Fluoride coat wipes off → glass not hot enough.

Dangers

Danger Implosion. An evacuated bell jar carries a tonne of air pressure on its surface. A scratch, a knock or a hot spot can burst it inward and spray glass. Inspect it before every run; keep a wire-mesh guard or a cloth wrapping round it; wear goggles; never set anything on top of it.

Danger High voltage. The glow-cleaning and sputtering supplies kill. Interlock them so they cannot be on while the jar is open, and discharge everything before you touch it (Wiring and Electrical Safety).

  • Hot oil and air: venting a hot oil diffusion pump can start a fire. Mercury pumps release poisonous vapour if the trap warms up (Mercury).
  • Cold: dry ice and liquid air burn skin and, evaporating in a small closed room, drive out the oxygen (Liquid Air, Nitrogen and the Noble Gases).
  • Chemicals: sodium fluoride is a poison; sodium sulfide with any acid gives off hydrogen sulfide, which smells of rotten eggs at first, but at dangerous strengths deadens the sense of smell so you stop noticing it, and then kills. Make them outdoors. Never use thorium fluoride, found in old coating recipes: it is radioactive.

What this unlocks

Long-lasting The Telescope mirrors and bigger Building an Observatory instruments; bright, glare-free Photography, The Microscope and binocular optics; laser mirrors and filters (Lasers, The Spectroscope); chip wiring (Making Microchips); conductive glass for screens (Flat Screens: LCD and LED Displays); low-emission window glass (Window Glass, Insulation and Keeping Buildings Warm or Cool); mirror film for Solar Heat collectors and satellites.

How it was first done

William Grove saw metal sputtered from the cathode of a glow discharge in 1852, and Michael Faraday made thin metal films by exploding wires in 1857. In 1887 Richard Nahrwold evaporated platinum in a vacuum, and around 1900 Thomas Edison's laboratory used sputtered gold on wax phonograph masters. Hot-filament evaporation of metals was worked out in the 1910s and 1920s; in the 1930s John Strong at the California Institute of Technology perfected aluminising, and in 1935 coated the 2.5 m mirror at Mount Wilson. Alexander Smakula at Carl Zeiss in Jena patented anti-reflection coating in 1935, and it was kept a military secret for some years; Walter Geffcken at Schott made the first multilayer interference filters in 1939. Wolfgang Gaede had invented the diffusion pump in 1915, and Cecil Burch's low-vapour oils of 1928 made oil pumps practical. Multilayer laser mirrors followed in the 1960s, and magnetron sputtering in the 1970s.