◆ Rebuild

Part 3 · Metals

Electroplating

Use an electric current to lay a thin, even skin of one metal over another — copper, nickel, silver, zinc — to stop rust, add beauty or conductivity, or build up exact metal copies of a shape (electroforming). Plus hot-dip galvanising, the cheapest way to keep iron from rusting for decades.

Difficulty
●●●●●
Time
An afternoon for a first copper plate once you have copper sulfate and a battery; a day or two to electroform
Steps from zero
16 prerequisites →

You need first

ElectrolysisThe Battery

This unlocks

Anodising Aluminium and Titanium
The full path from nothing — 16 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Salt
  12. Fermentation
  13. Bellows
  14. Copper Smelting
  15. The Battery
  16. Electrolysis
  17. Electroplating

Do them roughly in this order. See it on the tech tree →

Why it matters

A coating a few hundredths of a millimetre thick can change what a metal is good for:

  • Rust protection. Nickel over copper over iron for tools, fittings and instruments; zinc for buckets, roofing, wire and bolts.
  • Conductivity and contacts. Silver and gold on switch contacts and connectors for the The Telegraph, The Telephone and Radio; tin or silver on copper wire so it solders easily.
  • Beauty and value. Silver-plated cutlery and dishes at a fraction of the cost of solid silver (Gold and Silver).
  • Wear. Hard nickel (and later chromium) on shafts and moving parts; worn parts built back up to size.
  • Copies. Electroforming grows a thick metal skin on a mould, making exact copies of printing plates (Printing), medals, records (Recording Sound) and fine parts.

Plating is one of the first practical uses of electricity, and among the easiest. A copper plating bath can run on a single home-made cell (see The Battery).

How it works

Plating is Electrolysis with a metal salt in the liquid.

  • The object to be plated hangs in the bath as the cathode — joined to the negative (−) terminal.
  • A bar or sheet of the plating metal hangs opposite as the anode — joined to the positive (+) terminal.
  • The liquid, the electrolyte, contains the plating metal dissolved as a salt — copper sulfate for copper, for example.

When current flows, metal from the liquid is laid down atom by atom on the object, and the anode dissolves at the same rate to replace it. The anode slowly wastes away; the object slowly grows.

+− Anode (+)pure copper; slowlydissolves Cloth bagcatches anode sludge Object (−)copper laid downon every face Bathcopper sulfate +sulfuric acid in water Resistorsets the current Battery or dynamo1–6 V, direct current copper travels to the object anode and object 5–15 cm apart
Fig. 1 The plating cell. Current flows from the positive pole through the anode, across the bath, and onto the object hung as the cathode. Copper dissolves from the anode and is laid down on the object.

How much metal

Faraday's law: the weight of metal laid down depends only on the current and the time.

Metal (bath) Grams per ampere-hour Thickness per hour at 1 A on 1 dm² (100 cm²) Usual current density
Copper (acid sulfate) 1.19 13 µm 1–4 A/dm²
Nickel (Watts) 1.09 12 µm 2–5 A/dm²
Silver 4.02 38 µm 0.2–0.5 A/dm²
Zinc (acid sulfate) 1.22 17 µm 2–5 A/dm²

A µm (micrometre) is a thousandth of a millimetre; a human hair is about 70 µm thick. A good protective nickel coat is 10–25 µm; good silverware carries 20–30 µm of silver.

Current density — amperes per area of the object — decides the quality. Too little and plating is slow. Too much and the coat comes out dark, rough and powdery ("burnt"), first at the edges and corners, which always get more current than flat faces. Measure the area of your object and set the current from the table: a plate 10 × 10 cm with both sides exposed is 2 dm², so for acid copper at 2 A/dm² it needs 4 A.

Measuring current without a meter

Put a copper coulometer in the circuit: a small jar of the copper bath with two clean copper strips, in series with your plating tank. Weigh the negative strip before and after (see Measurement from Scratch). Every 1.19 g it gains means one ampere-hour has passed. Divide by the hours to get amperes. A galvanometer (Measuring Electricity) once calibrated this way serves for years.

What you need

Item Notes
DC power 1–6 V at 1–20 A. One or two Daniell cells for small copper work (The Battery); a bank of cells or a low-voltage dynamo (The Generator) for larger work. Never AC.
Current control A coil of iron or German-silver wire with a sliding clip, or a carbon rod with a movable contact.
Tanks Glass, glazed stoneware (Stoneware and Porcelain), or wood lined with pitch or wax (Tar, Pitch and Glue). Size: room for the work with 5–10 cm all round.
Anodes Plates of pure copper, nickel, silver or zinc, with about the same area as the work.
Bus bars and hooks Copper rods across the tank; copper wire to hang the work.
Chemicals See each bath. Copper sulfate, sulfuric acid, nickel salts, boric acid, silver salts, lye or soda ash, hydrochloric acid.
Cleaning Sand, pumice or brick dust, a stiff brush, scratch-brush of fine brass or iron wire.
Water Rain water or distilled water (Distillation); hard well-water spoils baths.

Where to find it

Most of what you need is made, not found:

  • Copper sulfate ("blue vitriol"): heat scrap copper red-hot in air until it is covered in black scale, knock the scale off and dissolve it in warm dilute Sulfuric Acid (1 part acid to 5 of water); repeat until the acid will take no more. Boil down and let it cool: bright blue crystals grow. Natural blue crusts of copper sulfate also form in old copper mines. See Copper Smelting.
  • Nickel salts: dissolve nickel metal (see Nickel and Cobalt) in warm dilute sulfuric acid with a little Nitric Acid; boil down to green crystals of nickel sulfate. A little hydrochloric acid gives nickel chloride.
  • Boric acid: stir Hydrochloric Acid into a hot, strong solution of borax until it tastes sour; shiny flakes of boric acid crystallise as it cools. Borax comes from the crusts of dry desert lakes (see Borax and Boric Acid).
  • Silver salts: silver dissolved in Nitric Acid gives silver nitrate. See Silver Nitrate and Silver Salts and Gold and Silver.
  • Cleaning chemicals: lye from wood ash (Lye and Potash); soda ash (Soda Ash and Baking Soda); hydrochloric acid (Hydrochloric Acid).
  • Sand and brick dust for scouring; graphite and beeswax for electroforming.

Step 1: Preparing the surface

Nine plating failures out of ten are dirty surfaces. A coat on grease or oxide peels off like sunburnt skin.

cleangreasysheetdrops 1. Scourwet sand, thenbrick dust 2. Degreasehot lye or soda,10–20 minutes 3. Water testdrops = grease:go back to 2 4. Pickledilute acid,1–5 minutes 5. Rinseclean water;no fingers now 6. Platein at once,with current on
Fig. 2 Preparing the work. Scour it bright, degrease it in hot lye, rinse, and check that water sheets evenly over it. Pickle off the oxide in dilute acid, rinse again, and hang it in the bath at once.
  1. Make it smooth. Plating copies every scratch. File, scour with wet sand, then fine brick dust or pumice, until the surface is as smooth as you want the finished piece.
  2. Degrease. Scrub with a hot solution of lye or soda ash (about 50–100 g per litre) and a stiff brush, or simmer the piece in it for 10–20 minutes. A paste of chalk (whiting) and water rubbed on with a rag also works.
  3. Rinse in clean running water.
  4. The water-break test. Lift the piece out. On a clean surface the water spreads in an unbroken sheet. If it pulls back into drops or dry islands, there is still grease: degrease again. From now on, do not touch it with your fingers; handle it by the hanging wire.
  5. Pickle to remove the thin oxide film:
    • Iron and steel: dip in dilute hydrochloric acid (1 part to 2–3 of water) or sulfuric acid (1 part to 10 of water) for 1–5 minutes, until evenly grey with no rust spots.
    • Copper and brass: a few seconds in dilute sulfuric acid, until evenly pink or yellow.
  6. Rinse again and go straight into the bath, with the current already switched on.

Step 2: The baths

Always add acid slowly to water, never water to acid. Mix baths in glass or stoneware.

Acid copper

Water Copper sulfate crystals Sulfuric acid (concentrated) Temperature Current Voltage
1 litre 200 g 50 g (about 27 mL) Room temperature 1–4 A/dm², start at 2 0.5–1.5 V

Use copper anodes, wrapped in a bag of tightly woven cloth to catch the sludge that falls from them. At 2 A/dm², the coat grows about 25 µm an hour. Stir or rock the work gently now and then.

The acid copper bath cannot plate iron, steel or zinc directly: those metals push copper out of solution by themselves and become covered with a loose, powdery copper film that rubs off. Give iron a thin coat of nickel first, then copper. (Factories used a cyanide copper bath for this — see the dangers.)

Nickel (the Watts bath)

Water Nickel sulfate Nickel chloride Boric acid Temperature Current Voltage
1 litre 250–300 g 40–50 g 30–40 g 45–60 °C (too hot to keep a finger in) 2–5 A/dm² 3–6 V

Use nickel anodes. The bath should be slightly acid: it should turn blue litmus paper slowly red (see Acids, Bases and Testing); add a few drops of sulfuric acid if not. Nickel plates directly onto clean steel and copper. Plate 10–25 µm for rust protection — 1–2 hours at 2–3 A/dm². The coat comes out dull grey-white and polishes to a bright mirror on a cloth wheel with fine abrasive (Abrasives and Grinding Stones).

For rust protection on steel, the best order is: nickel strike (thin), copper (thick, fills scratches), nickel (finish).

Silver

The classic silver bath of 1840 onward used potassium cyanide, and still gives the best results. Cyanide is one of the deadliest poisons there is (see the dangers). A cyanide-free alternative, used in reduced form here, is the thiosulfate bath — the same "hypo" used in Photography:

  1. Dissolve silver nitrate in water and add salt water (Salt) until no more white silver chloride settles out. Wash the white powder several times.
  2. Dissolve 250 g of sodium thiosulfate in 1 litre of water, and stir in the silver chloride from about 30 g of silver until it dissolves.
  3. Plate at 0.2–0.5 A/dm², about 0.5–1 V, with a silver anode, at room temperature.

Work slowly: high currents give dark, loose deposits. Copper and brass objects should go in with the current on, as with copper on iron. Traditional silverware is silver plated onto nickel silver, a white alloy of copper, nickel and zinc — hence "EPNS", electroplated nickel silver.

Gold

Gold plating is usually only a flash 0.1–1 µm thick — enough for colour and for electrical contacts that must never tarnish. The traditional baths are cyanide; the old method of fire gilding used gold dissolved in mercury, and blinded and poisoned generations of gilders. Modern cyanide-free gold baths, based on sodium sulfite, exist but need careful chemistry. Treat gold plating as a task for a skilled chemist, and use silver or nickel where you can.

Step 3: Plating

  1. Hang the cleaned work on copper wire from the negative bus bar, and the anodes from the positive bar, 5–15 cm apart, facing the work on both sides if it has two faces.
  2. Set the current from the area and the table above. Start low and increase.
  3. Watch. A fine, even, matt colour should spread over the whole piece within a minute. A few fine bubbles on the work are normal in nickel baths; streams of bubbles mean the current is too high.
  4. Time it from Faraday's law for the thickness you want.
  5. Take it out, rinse, and dry it in warm sawdust or with a soft cloth. Polish if wanted.

Electroforming: making metal copies

This is how printing plates (electrotypes), medals, and fine metal shapes were copied from the 1840s on.

  1. Make a mould. Press the original — a woodcut, a page of type, a coin — into warm beeswax (or a mixture of wax and a little resin), or cast plaster of Paris (Gypsum and Plaster of Paris) round it and seal the plaster with hot wax.
  2. Make it conduct. Brush the face of the mould with the finest graphite powder until it shines like dark metal everywhere. Press a bare copper wire into the edge of the wax so it touches the graphite.
  3. Plate in the acid copper bath at 1–2 A/dm². Copper creeps in from the wire over the graphite; when the whole face is covered, keep going.
  4. Build it up for 1–3 days, to 0.3–1 mm thick.
  5. Separate the copper shell by warming the wax in hot water. For a printing plate, back the shell with molten type metal (Lead) to stiffen it.

Hot-dip galvanising

Galvanising is coating iron with zinc. Zinc corrodes before iron does — it sacrifices itself — so even where the coating is scratched, the iron underneath does not rust. Galvanised iron lasts 20–50 years outdoors where bare iron would rust through in a few. Electroplating zinc is possible (an acid zinc sulfate bath, 2–5 A/dm²), but the thicker, cheaper and older way is to dip the iron in molten zinc (see Zinc and Brass).

  1. Clean the iron as above, then pickle in hydrochloric acid until all rust and scale is gone, and rinse.
  2. Flux. Dip it in a hot strong solution of zinc ammonium chloride (zinc dissolved in hydrochloric acid, with sal ammoniac — ammonium chloride — added; see Ammonia), and let it dry completely in a warm place.
  3. Melt the zinc in an iron pot to 445–465 °C. That is just above zinc's melting point (420 °C): it shows no glow, but is fully liquid and runny, and a dry pine shaving dropped on it chars black within seconds. Skim the oxide off the top.
  4. Dip the dry work in slowly. It bubbles and spits as the flux burns off. Leave it until the bubbling stops and the iron is as hot as the zinc — 1–5 minutes.
  5. Withdraw it slowly, shaking or tapping off the extra zinc, and let it cool in air (or quench in water once it is out and the zinc has set).

A good coat is 50–100 µm, bright and spangled like frost when new, dull grey later.

How to tell it worked

  • Look. An even colour all over, with no bare spots, dark burnt edges or blisters.
  • Bend test. Plate a strip of scrap with the same piece. Bend it double: the coat should crack or stretch with the metal, never flake off.
  • Heat test. Heat a plated sample to about 200 °C (a pine stick laid on it just starts to brown) and drop it into cold water. Poorly bonded coats blister.
  • File test. File the edge from the base metal toward the coat. A good coat does not lift.
  • Weight. Weigh the piece before and after: the gain divided by the area and the metal's density gives the thickness.
  • Rust test (for nickel and zinc on iron): a week in damp salty air shows no rust spots.

Note Troubleshooting. Object dissolves instead of plating → wires reversed. The work must be on the negative (−). Coat peels or blisters → grease or oxide: repeat the water-break test, pickle, and enter the bath with current on. On iron in copper: nickel first. Dark, rough or powdery, especially at edges → current too high. Lower it, or move the anodes further away. Pitted with tiny holes → bubbles clinging. Rock the work; keep the bath clean. Rough, gritty coat → sludge from the anode. Bag the anodes; filter the bath through cloth. Nickel dark, cracked or streaky → bath too cold, or not acid enough, or impure. Warm it, check acidity, add boric acid. Galvanising patchy, with black bare spots → flux missing or wet, or iron not pickled clean.

Dangers

Danger Cyanide. The historical baths for copper on iron, silver and gold used potassium or sodium cyanide. A few hundred milligrams kill an adult, and any acid — even pickling acid on a wet object — releases hydrogen cyanide gas from it, which kills in minutes. This book does not give cyanide bath recipes. Use the cyanide-free methods here.

Danger Acids. Concentrated sulfuric acid boils and spits if water is poured into it. Always add acid slowly to water, stirring. Wear eye protection and keep plenty of water and some soda ash nearby to wash and neutralise spills. See Acids, Bases and Testing.

Danger Molten zinc and water. A wet object dipped in molten zinc explodes into steam and throws zinc. Dry the work completely. Zinc fumes cause metal-fume fever; galvanise outdoors.

  • Nickel salts cause stubborn skin rashes in many people, and are suspected of causing cancer. Wear gloves; wash; do not breathe the spray from a gassing bath.
  • Chromium plating uses chromic acid, a poison that causes cancer and deep skin ulcers. It needs proper chemical training and ventilation (see Chromium and Its Compounds).
  • Hydrogen bubbles from plating tanks, especially nickel and zinc. Keep flames away and ventilate.
  • Mercury fire gilding and mercury "quicking" dips were once common: never use them. See Mercury.
  • Spent baths poison fish and soil. Recover the metal (by plating it out onto scrap) before disposing of the liquid far from wells and streams.

Going further

How it was first done

In 1805 the Italian chemist Luigi Brugnatelli, a friend of Alessandro Volta, gilded two silver medals using Volta's new pile. In 1838 Moritz Jacobi in St Petersburg, and in 1839 Thomas Spencer in Liverpool, independently copied engraved plates and medals by depositing thick copper — the birth of electroforming. In 1840 the cousins George and Henry Elkington of Birmingham patented silver and gold plating with cyanide solutions, using the discovery of a local surgeon, John Wright, that silver dissolved in potassium cyanide gave fine coats. Elkington's works installed one of the first generators used in industry, a magneto built by John Stephen Woolrich, in 1844. Rudolf Böttger in Germany plated nickel in 1842, and Oliver Watts in the United States published the nickel bath that bears his name in 1916. The French chemist Paul Jacques Malouin described coating iron with molten zinc in 1742, and Stanislas Sorel patented hot-dip galvanising in France in 1837.