◆ Rebuild

Part 3 · Metals

Presses, Punches and Dies

A hardened steel punch driven through sheet into a matching die cuts, bends, cups or stamps a part in one stroke, identical every time. How to build a fly press and a coining screw press, make punch-and-die pairs for blanking, piercing, bending and deep drawing, chain them into a progressive die, and strike coins and medals — the way buttons, eyelets, can ends, pen nibs and clips are made by the million.

Difficulty
●●●●●
Time
Weeks to build a fly press; one to three days to make a simple punch and die; then a part every few seconds
Steps from zero
19 prerequisites →

You need first

Screws, Nuts and BoltsSteelSheet Metal and Rolling

This unlocks

—
The full path from nothing — 19 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Fire
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Hides and Leather
  10. The Wheel and Axle
  11. Bellows
  12. The Lathe
  13. Gears
  14. Iron (the Bloomery)
  15. The Waterwheel
  16. Blacksmithing
  17. Steel
  18. Sheet Metal and Rolling
  19. Screws, Nuts and Bolts
  20. Presses, Punches and Dies

Do them roughly in this order. See it on the tech tree →

Why it matters

Snips and a hammer make one bracket in ten minutes. A punch and die makes it in two seconds, and the ten-thousandth matches the first. That is mass production in thin metal. Buttons, eyelets, washers, hinges, lock parts, lamp burners, can ends and bottle caps, pen nibs, spring clips, clock wheels, electrical terminals, the laminations of every The Transformer and The Electric Motor, the shells of lamp burners and gauges: all are pressed.

A press also strikes coins. Hammer-struck coins (Money, Trade and Record-keeping) are uneven and easy to forge; coins struck in a screw press inside a collar are perfectly round, with a sharp design and a milled edge that shows any clipping.

Hot forging between dies belongs with Blacksmithing and Machine Tools; spinning hollow shapes is in Metal Spinning and Raising.

How it works

Shearing. A punch pressing sheet into a sharp-edged die hole dents it, cuts a little way in, then cracks the rest. Cracks run from the punch edge and the die edge toward each other. With the right gap between them — the clearance — they meet cleanly. Too little and they miss, leaving a torn double edge and fast tool wear; too much and the metal is dragged into the gap, leaving a big ragged burr (a sharp raised lip).

Sheet Clearance on each side, as a share of thickness
Lead, tin, soft aluminium 3–5%
Copper, soft brass 4–6%
Mild steel, wrought iron 6–8%
Hard brass, spring steel 8–10%

For 1 mm mild steel that is about 0.07 mm a side — about the thickness of a sheet of thin writing paper.

Which tool sets the size. For the piece that falls through (a blank), make the die hole to size and the punch smaller by the clearance. For a hole (piercing), make the punch to size and the die larger.

Force. The force to shear a shape is its outline length × the sheet thickness × the shear strength of the metal. Shear strength, roughly: lead 20 N per mm², aluminium 70–100, copper 150–200, brass 250–300, mild steel 300–350. A 25 mm disc (outline 79 mm) from 1 mm mild steel needs 79 × 1 × 320 ≈ 25,000 N — about 2.5 tonnes. A 100 mm disc from 2 mm steel needs 20 tonnes. Always work this out before you make the tool.

Drawing. A blank pushed by a round punch through a round die with a rounded mouth becomes a cup. The rim shrinks as it is pulled in, so it wrinkles unless a blank holder presses it flat while it slides. The metal flows in from the rim rather than stretching, so the wall keeps about the sheet's thickness. One stroke can make a cup about half the blank's diameter; deeper cups need redrawing in steps, annealed between.

Coining squeezes metal in a closed die until it flows like stiff clay into every hollow — tens of tonnes for a coin.

What you need

Item Notes
Tool steel High-carbon steel, 0.9–1.2% carbon, or a tungsten or chromium tool steel (Alloy and Stainless Steels). Old files are excellent once annealed (Files and Saws).
A press A fly press for most work up to 1.5 mm; a big screw press, drop hammer or hydraulic press for heavy blanking and coins. Built below.
Machine tools A lathe for round punches and dies (The Lathe, Machine Tools); a drill, files, scrapers, a vice, a surface plate.
Hardening A forge or muffle that reaches cherry red evenly, water or oil for quenching, a plate for tempering (Steel, Forge Shops and Heat Treatment).
Measuring Calipers, a micrometer if you have one, feeler gauges cut from thin shim (Rules, Squares, Callipers and Gauges, Scientific Instrument Making).
Sheet and strip Annealed brass, copper, tinplate, mild steel, cut into strips (Sheet Metal and Rolling, Tin and Pewter).
Lubricant Tallow, lard, soap solution or thin vegetable oil for drawing; a drop of oil on blanking strip.

Where to find it

All of it is made, except hardwood for bases and handles and animal fat or plant oil for lubricant (Oils and Pressing). Steel comes from Steel and Steel in Quantity, the frame from The Blast Furnace and Cast Iron, the nut from Bronze.

The presses

Fly press

The press of every small metal shop for two hundred years: a heavy C-shaped frame with a vertical screw driving a guided ram that carries the punch. On top of the screw sits the fly, a bar 1–1.2 m long with a heavy ball at each end. Swing it a quarter or half turn; the balls store your effort and spend it in the last few millimetres. One person strikes 10–20 parts a minute.

Fly ball 10–30 kg each Handle swing ¼–½ turn Cast-iron frame throat 15–25 cm Timber block Fly arm, 1–1.2 m Stop collar sets stroke depth Bronze nut cast into the frame Multi-start screw 40–80 mm per turn Ram in guide Punch Sheet strip Die in bolster clamped to the bed
Fig. 1 The fly press. Swinging the weighted arm turns a steep, multi-start screw, which drives the ram down. The punch is held in the ram; the die sits in a bolster on the bed.
Part Typical size (small to medium press)
Frame Cast iron, throat 15–25 cm deep, bed 25 × 20 cm, height 60–90 cm, weight 100–300 kg
Screw 40–75 mm diameter, three or four starts (several threads wound side by side) so it moves 40–80 mm per turn
Nut Bronze, cast or pressed into the frame top, length 1.5× the screw diameter
Ram Square or round, 50–75 mm, sliding in a long guide with adjustable strips; a 16–25 mm hole in its foot for the punch shank, held by a set screw
Fly balls 10–30 kg each
Stop A collar on the screw that limits the stroke, so the punch stops just inside the die

Building one. Cast the frame in grey iron, ribbed, with at least 5 cm of metal at the throat corner where it tries to open (Metal Casting); small presses can be forged wrought-iron bars bolted together. Cut the screw on a screw-cutting lathe (Screws, Nuts and Bolts), one start at a time, turning the work exactly 1/3 or 1/4 turn between starts. Cast the bronze nut round the greased screw. Plane the ram and guide square to the bed (Machine Tools) so the punch lands in the same place every stroke. Bolt the frame to a heavy block at waist height.

A counterweight or spring lifts the ram after each blow, leaving one hand free to feed.

Screw press for coins and heavy work

The coining press, or balancier, is the fly press grown large: an arch frame, a screw 10–15 cm across and an arm 2–3 m long with 50–200 kg weights, pulled round by two to four people with straps. It delivers the tens of tonnes coins need.

Other presses, in brief

  • Drop hammer — a weight lifted by rope or cam and dropped onto the upper die. Powerful but hard to control.
  • Crank press — a flywheel, belted from a line shaft or The Electric Motor (Belts, Chains and Power Transmission), drives the ram through a crank once a turn when a pedal trips the clutch: 30–100 strokes a minute. The factory blanking press.
  • Hydraulic press (Hydraulic Presses and Rams) — slow, enormous force, for deep drawing, large panels and coining.

Punches, dies and die sets

Punch smaller by the clearance Stripper plate pulls strip off punch Sheet strip Die block hole = blank size Bolster Clearance 4–8% of thickness a side Straight land 2–3× thickness Relief taper 1–2° each side Blank falls through The cut edge of a blank, greatly enlarged shiny tiny burr Right clearance shiny band ⅓, clean break Too much clearance rolled edge, big burr Too little clearance two shiny bands, fast wear
Fig. 2 A blanking tool in cross-section, and the cut edge it leaves. The die hole sets the blank size; the punch is smaller by the clearance. The stripper pulls the strip off the punch on the way up. The hole tapers below a short straight land so blanks fall through.

Simple punch and die

The first tool to make: round, for washers and discs.

  1. Anneal a piece of tool steel 25–30 mm thick for the die block, and a round bar for the punch (heat cherry red, cool slowly in ash).
  2. Bore the die. Drill and bore the hole to the blank size. Keep it dead straight for a land of 3 mm (2–3× the sheet thickness) below the top face; then open it out underneath with a taper of 1–2° per side, so the cut pieces fall through instead of jamming.
  3. Turn the punch to the hole size minus twice the clearance, with a shank to fit the ram. Keep its face flat and its edge sharp and square. Its working length should be no more than 3–4 times its diameter, or it buckles.
  4. Fit before hardening. Push the punch into the die by hand from the top. It should enter with an even, just-visible gap all round when held up to the light. File or lap any tight side.
  5. Harden both in water or brine from cherry red (about 780–800 °C, when a magnet no longer sticks). Temper: the die to pale straw (about 220 °C), the punch to dark straw or brown (240–260 °C) so it is a little tougher than the die (Steel).
  6. Grind the faces flat on a fine stone or surface grinder to bring the edges back sharp.

For other shapes, file the die hole to a scribed outline and a hardened template. Then harden the die, make the punch a hair too big, smear it with soot in oil and press it lightly into the die; the shiny spots show where to file. Never force a hardened punch through a hardened die — one will crack.

Stripper and guides

As the punch comes up, the springy sheet clings to it. A stripper — a steel plate fixed 1–2 mm above the die, with a hole a little larger than the punch — catches the strip and pulls it off. Between the stripper and die, two guide strips keep the strip running straight, and a stop pin sets how far you advance it each stroke.

Die set

A slack ram lets the punch wander and chip. A die set cures it: two thick plates joined by two hardened guide pillars sliding in long bushes. The bottom plate is bolted to the bed, the ram drives the top plate through a loose shank, and the pillars — not the press — keep the punch centred. Worn presses with good die sets made Precision and Interchangeable Parts.

Blanking and piercing

  1. Work out the force. Make sure the press can give at least 1.5 times it.
  2. Set the die on the bed, bring the punch down slowly by hand into the die about 1 mm, and clamp the die there. Raise the punch and set the stroke stop so it enters 0.5–1 mm past the bottom of the sheet and no more.
  3. Feed annealed strip, oiled lightly, against the stop. Strike. Advance. Strike.
  4. Layout. Leave a bridge of metal between neighbouring blanks and at the strip edges of at least the sheet thickness, and never less than 1 mm. For round blanks, stagger two rows in a wide strip to save metal.

Shaving. For parts that need a clean, square edge (clock wheels, gauge parts), blank a little oversize and push the blank through a second die only 0.05–0.1 mm smaller. The shaving die trims off the torn part as a fine curl.

Bending

A bending die is a V-shaped groove with a wedge punch, or a U-shaped channel with a square punch.

  • V-die opening: 6–8 times the sheet thickness for steel, 5–6 for soft brass and copper.
  • Inside bend radius: at least the sheet thickness for mild steel, half that for soft copper, 2–3 times for spring steel and hard brass. Sharper and the outside cracks.
  • Springback: metal opens a little when released. Make the V a few degrees sharper than you want — 86–88° for a 90° bend in mild steel, 84–86° in brass — or let the punch strike the bottom of the V hard (bottoming), which sets the bend.
  • Grain: rolled sheet bends more safely across its rolling direction than along it.

A long V-die and blade is a press brake for the edges of tanks and ducts (Tins, Cans, Drums and Tanks). A curling die rolls an edge into a tube in a curved groove, for hinges and can ends.

Deep drawing

1. Blank on the die 2. First draw 3. Redraw Blank holder springs Blank Punch Die mouth radius 5–10× thickness Cup ≥ half the blank rim slides in; wall keeps its thickness Anneal, then a smaller die each step ≥ 0.75 of the last
Fig. 3 Deep drawing. The blank holder presses the rim flat while the punch pulls the centre down through the die; the rim slides inward and becomes the wall. A deep cup is made in two or more draws, annealed between them.

The drawing die makes cups, cans, lamp burner shells, thimbles, eyelets, lamp sockets and sinks.

Rule Value
Blank diameter for a flat-bottomed cup D = √(d² + 4·d·h), where d is the cup diameter and h its height
First draw Cup at least 0.5–0.55 of the blank diameter
Each redraw Cup at least 0.75–0.8 of the previous one
Die mouth radius 5–10 times the sheet thickness
Punch nose radius 4–10 times the thickness
Clearance (each side) 1.1–1.2 times the thickness (more than for cutting — the wall must pass)
Best metals 70/30 brass (cartridge brass, Zinc and Brass), soft copper, aluminium, tinplate, very soft low-carbon steel

Example: a cup 30 mm across and 30 mm deep needs a blank √(900 + 3,600) ≈ 67 mm. That is 2.2 times the cup — too much for one draw. Draw first to 38 mm (67 ÷ 38 = 1.76), anneal, then redraw to 30 mm.

Steps.

  1. Turn the die with a polished, rounded mouth, and the punch to the cup's inside diameter with a small vent hole so the cup does not suck onto it.
  2. Make the blank holder: a ring on the die face round the punch, pressed down by stiff springs, rubber or hand-set bolts. Too light — wrinkles; too heavy — the bottom tears out.
  3. Grease both sides of the blank with tallow or soap-and-oil paste.
  4. Centre the blank, close the holder, and draw in one steady stroke. A slow screw or hydraulic press beats a fly press here: the metal needs time to flow.
  5. Anneal brass and copper between draws; pickle off the scale (Acids, Bases and Testing).
  6. Trim the uneven rim (ears) in a lathe or trimming die.

Ironing. Push the cup through a die slightly smaller than its outside so the wall is squeezed thinner and longer. This is how tall thin-walled cases and cans are made from short cups.

Progressive and compound dies

A progressive die does several steps on one strip, one station after another. Each stroke advances the strip one pitch (the distance between parts) and every station works at once, so a finished part drops out every stroke.

Example: a washer 20 mm outside, 10.5 mm hole, from 1.5 mm strip 23–24 mm wide.

  1. Station 1 pierces the 10.5 mm hole.
  2. The strip moves on one pitch, 21.5 mm (20 mm blank + 1.5 mm bridge).
  3. Station 2 blanks the 20 mm outside. A rounded pilot pin on the blanking punch, a shade under 10.5 mm, enters the pierced hole first and pulls the strip into exact place, so the hole ends up centred.

Draw the strip full size on paper first, with every station and pilot; leave an idle station between two close holes so the die block is not too thin. A compound die pierces and blanks at one station in one stroke — flatter parts, but harder to make.

Coining and medals

How a coin is designed, weighed and accounted for is in Money, Trade and Record-keeping. Here is how it is struck.

The blank (planchet). Blank discs from strip rolled to exact thickness; weigh a sample and adjust the rolling until the weight is right. Roll each blank along a groove between two steel faces (upsetting) to thicken its edge into a slight rim. Anneal and clean bright in weak acid.

The dies. Cutting every die by hand means no two match. Hubbing makes them identical:

  1. The engraver cuts the design sunk and in reverse in a soft steel blank — the matrix (Engraving, Seals and Etching). Harden it.
  2. Press the hardened matrix into a soft steel blank in the screw press, several blows with annealing between, to make a hub: the design in relief, the right way round. Harden it.
  3. Press the hub into as many soft working die blanks as you need. Each one is identical. Harden and temper them to straw. The die faces are given a very slight dome (a few hundredths of a millimetre), which helps the metal flow to the rim.

The collar. A hardened steel ring round the lower die. The struck blank spreads to fill it exactly, so every coin is the same size and perfectly round; fine grooves inside it give a reeded (milled) edge. The lower die rises to push the coin out.

Striking. A copper, brass or cupronickel coin 25 mm across needs about 40–60 tonnes; soft silver less; gold least. Low relief (0.1–0.2 mm) strikes up in one blow. Medals with high relief (1–3 mm) take several blows, annealing the medal between them; each blow must land with the medal in exactly the same position in the collar. See Jewellery, Beads and Medals for finishing medals and badges.

Pressed objects

Eyelet. Blank a 10 mm disc from 0.3–0.4 mm brass, draw it into a cup about 5 mm across and 4 mm deep in two draws, pierce out the bottom, leaving a 1 mm flange, and run it through a flaring punch to turn the flange flat. The barrel goes through the cloth, leather or card from the front; an eyelet setter — a punch with a rounded, pointed nose and a dished anvil — splits and rolls the barrel back over the other side. A good eyelet is round, rolls without splitting raggedly, and cannot be turned in its hole.

Buttons are blanked, domed and closed in three or four dies (Buttons, Buckles, Hooks and Zips); can ends and bottle caps blanked, ringed and curled in one die (Tins, Cans, Drums and Tanks); pen nibs blanked, pierced, raised, hardened, then slit (Pens, Nibs and Writing Instruments); spring clips blanked and bent soft from spring-steel strip, then hardened and tempered blue (Springs); laminations blanked from silicon-iron sheet in progressive dies (The Transformer).

How to tell it worked

  • Cut edge. Look at a blank's edge with a lens. A good edge has a smooth, shiny burnished band about a third of the thickness, then a dull, slightly sloping break, and only a tiny burr. A big burr means too much clearance or a dull punch; two shiny bands mean too little clearance.
  • Size. Measure the first, the hundredth and the thousandth part. When they creep up (blanks) or down (holes), the edges are wearing: grind the faces.
  • Drawn cups have even walls (check with calipers at four points), no wrinkles in the flange, and no cracks at the bottom corner.
  • Coins show the full design to the edge, crisp letters, a sharp rim, and weigh within the set tolerance. Two coins from the same dies look identical side by side.

Note Troubleshooting. Blanks stick in the die and pile up → no relief taper below the land, or the land too long; re-cut the taper. Punch chips at the edge → punch and die misaligned, too hard, or striking too far into the die. Use a die set, temper the punch a little darker, set the stop. Ragged edge, big burr → clearance too large or the edges dull. Grind the faces; if still bad, make a new punch to fit. Cup wrinkles round the rim → blank holder too light, or the draw too deep for one step. Cup bottom tears out → blank holder too tight, die radius too sharp, poor lubrication, or the metal needs annealing. Coin design weak at the edge → not enough force, or the die faces too flat. Strike harder or give the dies a slight dome. Die cracks across → overheated in hardening, or a sharp inside corner. Round inside corners at least 0.5 mm.

Dangers

Danger Presses take fingers. Every press in history has crushed hands, because the operator's hand is under the punch hundreds of times a day and a lapse comes eventually. Never put a hand between punch and die. Feed strips long enough to hold from outside, or push blanks in with a wooden or brass stick, or use a sliding feed plate. Fit a guard round the punch that leaves room only for the sheet. Powered presses need a two-handed start (both hands on two separate levers to trip the clutch) or a guard that must close before the stroke. Stop when you are tired.

Warning Hardened steel shatters. A cracked die or a punch striking the die face can burst and throw fragments. Wear eye protection and stand to the side of a heavy press. Ring every die before use: a hardened die block hung on a wire and tapped should ring clear; a dull note means a crack.

  • Fly press arms swing through head height. Keep others clear of the circle.
  • Pickling acids used to clean annealed parts burn skin and eyes (Acids, Bases and Testing).

What this unlocks

Presses make Precision and Interchangeable Parts cheap: lock and clock parts (Locks and Keys, Clockwork, Music Boxes and Counting Machines), The Sewing Machine parts, The Bicycle fittings, the laminations of The Transformers and The Generators, lamp bases (The Light Bulb), terminals and tags (Building Circuits: Boards, Connectors and Cables), stamped car bodies (The Motor Vehicle) and sheet-metal kitchenware (Pots, Pans and Kettles). Coining presses give honest money (Money, Trade and Record-keeping). Shallow forming in dies is half of Tins, Cans, Drums and Tanks; the other route to hollow shapes is Metal Spinning and Raising.

How it was first done

Coins were struck by hand between two dies from about 600 BC in Lydia and Greece until the 1500s. In the 1550s the French king Henri II set up a mint in Paris with machines from Augsburg in Germany: a water-driven rolling mill for strip, a press to cut blanks, and a screw press for striking. The new machine-made coins were better, but the old hammer-men's guilds fought them, and in France and England hammering went on into the 1600s. England changed to screw presses for good in 1662.

In the 1780s–90s Matthew Boulton at Soho, Birmingham, drove screw presses with a The Steam Engine and struck Britain's "cartwheel" pennies of 1797, helped by the Swiss engraver Jean-Pierre Droz's work on collars and die-making. From about 1817 Diedrich Uhlhorn's self-feeding toggle press began to replace the screw press in mints.

Birmingham's "toy trade" stamped buttons, buckles and trinkets by the million on fly presses, and steel pen nibs from the 1820s–30s (Josiah Mason, Joseph Gillott). The crank press, progressive die and die set grew up with American interchangeable manufacture in the later 1800s.

Source: content/entries/metals/press-tools-and-dies.md