◆ Rebuild

Part 2 · Earth and Fire

Gypsum and Plaster of Paris

Gypsum is a soft white mineral that, gently heated to about 150 °C, becomes plaster of Paris — a powder that sets hard in minutes when mixed with water, copying every detail of a mould. For moulds and casts, smooth indoor walls, splints for broken bones, and the setting control in cement.

Difficulty
●●●●●
Time
An afternoon to cook a batch; minutes to set; a day or two to dry
Steps from zero
3 prerequisites →

You need first

The Kiln

This unlocks

Stairs, Floors and Interior FinishesSlip Casting, Jiggering and Ceramic Factories
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Gypsum and Plaster of Paris

Do them roughly in this order. See it on the tech tree →

Why it matters

Plaster of Paris is the easiest "artificial stone" there is. It needs only the heat of a cooking fire, sets hard in 10–30 minutes, and copies the finest detail — a fingerprint, a coin, the grain of wood. It is used for:

Gypsum needs far less heat than Lime (150 °C against 900 °C), so if you find it, plaster is one of the first building materials you can make.

How it works

Gypsum is calcium sulfate with water built into its crystals — two molecules of water for every one of calcium sulfate (chemists write CaSO₄·2H₂O). Water makes up about a fifth of its weight.

Gypsumcalcium sulfate + waterlocked in the crystals Heat gently: 120–180 °Cthree-quarters of the water leaves as steam loses 15–16% of its weight Plaster of Parisfine white powder Add watersets in 10–30 minutes,warms, swells slightly Set plastergypsum again: interlockingneedle crystals Crush andre-cookold plaster works again Too hotover 400 °C Dead-burntwill not set
Fig. 1 The plaster cycle. Gentle heat drives three-quarters of the water out of gypsum, leaving plaster of Paris. Adding water puts it back, and the crystals regrow as solid gypsum. Too much heat drives all the water out and "kills" the plaster.
  1. Calcining (cooking). Heated to about 120–180 °C, gypsum loses three-quarters of its water as steam and becomes a fine white powder: plaster of Paris (calcium sulfate hemihydrate, "half-water"). It loses about 15–16% of its weight.
  2. Setting. Mixed with water, the plaster dissolves slightly and immediately starts growing back into gypsum as a felt of tiny interlocking needle crystals. The mass sets solid in minutes and gets warm as it does. It expands very slightly (about 0.2–0.3%) as it sets, which pushes it into every detail of a mould.
  3. Drying. You always add more water than the reaction needs, to make a pourable paste. The extra water evaporates over a day or more, leaving tiny pores — this is why set plaster is light and soaks up water like a sponge.
  4. Overburning. Above about 200 °C the plaster loses all its water. Up to about 300 °C it will still take water back quickly. Above about 400–500 °C it becomes "dead-burnt" anhydrite that sets very slowly or not at all. (Gypsum burnt at red heat, 900–1,000 °C, makes a slow-setting but very hard floor plaster that was used in medieval Germany — a separate craft.)

Because the reaction runs both ways, plaster is a cycle: gypsum → plaster → gypsum. Old broken plaster can be crushed and re-cooked.

Gypsum dissolves slightly in water (about 2 grams per litre). Set plaster left out in the rain slowly washes away and goes soft when soaked. Use it indoors and in dry places only; outside, use lime (Lime) or cement.

What you need

Item Notes
Gypsum Clean white or grey lumps or crystals; about 1.2 kg makes 1 kg of plaster
Crusher Hammerstone or wooden pestle and a flat stone or wooden trough — gypsum is soft
Sieve Fine basket, or cloth stretched on a frame
Cooking vessel A wide, shallow iron pan or a thick clay pot or dish; for bigger batches an oven or kiln (The Kiln)
Stirring stick Hardwood, long-handled
Mixing bowl Flexible leather or rawhide bowls are ideal — set plaster cracks out of them
Water Clean and cool
Release agent Soft soap (Soap), oil, fat, or thin clay slip, to stop plaster sticking
Cloth Loosely woven cotton or linen strips for bandages; hair or fibre for wall plaster

Where to find it

Gypsum forms where salty water evaporates, so it is found with rock salt and in clays laid down in shallow seas and salt lakes.

  • Beds of white, grey, pinkish or brownish rock in layered sedimentary country, often with red and green clays and shales, sometimes forming low white cliffs and pitted, sinkhole-dotted ground (gypsum dissolves underground like limestone, but faster).
  • Clear crystals and glittering plates in clays and shales, especially where they have been dug or eroded.
  • Crusts and "desert roses" (rosettes of sand-filled crystals) in dry lake beds and deserts.
  • Around volcanic vents and hot springs, where sulfur fumes react with limestone.
  • Old buildings and ruins: drywall boards, plaster walls and plaster moulds are almost pure gypsum; crush and re-cook them. The from-scratch route is always the natural rock above.

Recognising it

Form Looks like
Selenite Clear, glassy plates that peel into thin, flexible sheets with a pearly shine; the sheets bend and stay bent or snap — unlike mica, which springs back
Satin spar White veins of parallel silky fibres
Alabaster Fine-grained, white or faintly coloured, translucent at the edges — prized for carving
Rock gypsum Massive, sugary or earthy white to grey rock

The tests (see Rocks and Minerals):

  1. Your fingernail scratches it (hardness 2). This alone rules out almost every other white mineral.
  2. It does not fizz with vinegar or acid. Calcite and limestone fizz, and they are too hard for a fingernail.
  3. It does not taste salty — unlike rock salt, which also scratches easily.
  4. Heat a flake on a hot stone or in the edge of a fire for a few minutes: gypsum turns opaque chalky white, gives off steam, and crumbles to powder between your fingers. Then mix that powder with a few drops of water: if it warms slightly and sets hard in 10–30 minutes, you have plaster.
  5. Anhydrite — gypsum's waterless cousin, found with it — is harder (a fingernail does not scratch it; copper does), heavier, and does not turn chalky or set. Sort it out.

Step by step: making plaster

  1. Clean and sort. Knock off clay and dirt. Pick out pieces of limestone (fizzes), anhydrite (hard) and sand.
  2. Crush. Pound to pieces no bigger than a pea, then grind to a coarse powder. Gypsum is soft, so this is easy. Sieve out lumps.
  3. Cook it. Put a layer 3–5 cm deep in a wide pan over a moderate fire, or in a pot set in hot embers. Stir constantly.
    • At first nothing happens. Then, at about 120–130 °C, the powder starts to "boil": it heaves, bubbles and flows almost like liquid as steam escapes. This is the water leaving.
    • Keep stirring and keep the heat steady and moderate. Do not let the pan glow.
    • After 30–60 minutes for a small pan, the boiling dies down and the powder settles and becomes still, soft and fine. That is the moment it is done. Take it off the heat.
  4. Judge the heat. No thermometer is needed: the bottom of the pan should be hot enough to make water drops spit and dance, but too cool to scorch a dry wood shaving brown quickly and far below any red glow. If a stick left resting on the powder blackens within a minute, it is too hot.
  5. For larger batches, use a bread oven (Cooking Without Pots) or a kiln. Heat the oven, rake out the fire, and load lumps of gypsum about 3–5 cm across; leave them several hours to overnight as the oven cools from about 250 °C. Or fire a pottery kiln very gently — well below any red glow — with gypsum on the cool upper shelves. Then crush and sieve the cooked lumps.
  6. Cool and store. Let it cool and sieve it fine. Store it dry, in a sealed pot, jar or barrel. Damp air slowly turns plaster back into gypsum, and it sets badly. Use it within a few weeks to a few months.

Mixing plaster

Add plaster to water — never water to plaster.

  1. Water first. Put cool, clean water in the mixing bowl. For a pourable mix use about 70 parts water to 100 parts plaster by weight (roughly 2 cups water to 3 cups plaster by volume). Less water gives harder, stronger plaster that sets faster; more gives weaker, softer plaster.
  2. Sift the plaster in by handfuls, scattered evenly over the surface, until little dry islands stop sinking and stand just above the water all over. This "island method" gives the right ratio without measuring.
  3. Let it soak for 1–2 minutes without touching it.
  4. Stir gently with your hand or a stick for 1–3 minutes, from the bottom, without whipping in air, until it is like thick cream with no lumps.
  5. Tap the bowl to bring air bubbles up, then pour or apply at once. You have perhaps 5–10 minutes before it begins to thicken. Once it starts to set, do not add water and re-stir — it will be weak and crumbly. Mix a new batch.
  6. Clean up before it sets. Never pour plaster or plaster water into a drain or a well; it sets there.

To slow it down (for wall plastering or large moulds), add a little hide glue dissolved in the water (Glues and Adhesives), or a dash of vinegar or sour fruit juice — test small amounts first. To speed it up, add a pinch of ground set plaster or a little salt, or use warm water.

Moulds and casts

1. First halfBury the original exactly halfwayin clay; press round hollows inthe clay; wall it in; pour plaster. 2. Second halfTurn it over, remove the clay. Thehollows are now keys. Soap well,three coats; pour the second half. 3. Open, cut a sprue, tieSeparate the halves, take out theoriginal, cut a pouring hole, andtie the halves shut with cord. plasterwooden wall soap on the parting face pour here
Fig. 2 A two-piece plaster mould. The original is half-buried in clay and the first half of the mould poured over it, with round "keys" scooped into the edge. After soaping, the second half is poured against the first; the keys make the halves lock back together exactly.

An open (one-piece) mould

For anything with a flat back — a tile, a medallion, a relief:

  1. Lay the original face up on a flat board. Coat it and the board thinly with soap, oil or fat.
  2. Build a wall of clay or wooden strips around it, 2–3 cm away and 2–3 cm higher than the original.
  3. Pour plaster gently into one corner so it flows over the original without trapping air. Brush the first thin layer into the details.
  4. After 30–60 minutes, when it is hard and has cooled again, remove the walls and pull out the original.
  5. Let the mould dry for a day or more before using it. For casting plaster or concrete in it, soap it well first.

A two-piece mould

  1. Bury the original exactly halfway in a bed of stiff clay. Smooth the clay surface right up to the original's widest line (the parting line). Press the round end of a stick into the clay at three or four places to make hollows.
  2. Wall around it and pour the first half of the mould. When set, turn it over and remove the clay. The hollows have become rounded bumps (keys).
  3. Soap the plaster face of the first half thoroughly (three coats, wiping off the excess); otherwise the two halves fuse together forever.
  4. Pour the second half against the first. When set, separate them, take out the original, and cut a pouring hole (the sprue) at one end.
  5. Tie the halves together with cord to cast.

What to cast in it

  • Plaster and concrete: soap the mould, pour, wait, open.
  • Wax: for figures and for lost-wax metal casting (Metal Casting).
  • Clay by pressing: press clay into a dry mould; the plaster soaks water out of the clay so it shrinks away and releases. Excellent for repeating tiles, handles and small items (Tiles and Clay Pipes).
  • Slip casting: pour liquid clay (slip) into a dry hollow mould; the plaster sucks water out of the slip, building a clay skin on the mould wall. After 10–20 minutes, pour out the extra slip, wait until the clay shrinks free, and open the mould. This makes thin, even pots, cups and laboratory ware (Stoneware and Porcelain); the full craft is in Slip Casting, Jiggering and Ceramic Factories.
  • Soft metals (lead, pewter, tin alloys): only in a mould that has been baked dry at 150–200 °C for several hours. Any water left in it turns to steam and can spit molten metal. For bronze and other hot metals, plaster must be mixed with fine sand or crushed brick — see Metal Casting.

Wall plaster

Gypsum plaster sets faster than lime and does not shrink, so it was used for smooth indoor walls from ancient Egypt onward.

  1. Base coat: 1 plaster : 2–3 sand by volume, with a handful of animal hair or chopped straw per bucket, 10–15 mm thick onto a damp wall. Roughen it with a stick.
  2. Finish coat: pure plaster, or 1 plaster : 1 lime putty (Lime), 2–3 mm thick, smoothed with a wooden or metal float as it begins to stiffen. Mixing in lime putty slows the set and makes the surface easier to polish. It also adds a little alkali, so the finish resists mould.
  3. Mix small batches — only what you can spread in 10–15 minutes — or add hide glue to slow it.
  4. Indoors only. On outside walls, damp walls, and near the ground, use lime or cement plaster.

Medical casts

A plaster cast holds a broken bone still so it can heal. Setting a bone properly is described in Emergencies and Basic Surgery; this is how to make the cast.

  1. Make bandages. Cut loosely woven cotton or linen into strips 8–15 cm wide and 2–3 m long. Rub dry plaster powder into the weave on a table and roll each strip up loosely. Store dry.
  2. Pad the limb. Wrap the limb in a smooth layer of soft wool, cotton or felt, extra thick over bony points (wrist, ankle, elbow, heel). Plaster must never touch skin directly.
  3. Wet one roll in a bowl of lukewarm water until bubbles stop (5–10 seconds), squeeze gently, and wrap it around the limb with each turn overlapping half the one before. Do not pull tight. Smooth each layer with wet palms so they bond. Use 6–8 layers; more at joints and across the sole.
  4. Hold the limb still in the right position for 10–15 minutes while it sets. Use flat palms, not fingertips — fingertip dents press into the skin.
  5. It reaches full strength in 24–48 hours as it dries. Keep it off the ground and dry, and do not let the person walk on a leg cast for two days.
  6. A simpler splint: a thick slab (10–12 layers) of plaster bandage laid along one side of the limb only and held with a cloth bandage. It leaves room for swelling and is safer when you cannot watch the patient closely.

Danger A tight cast can kill a limb. A broken limb swells in the first 1–2 days. If the cast is too tight, it cuts off blood. Check every few hours for the first two days: fingers or toes must stay pink, warm, able to move, and not numb. Severe pain, numbness, pins and needles, pale or blue fingers or toes are an emergency: cut the cast open along its full length at once, down to the skin and padding, and spread it apart. Do not wait.

How to tell it worked

  • Good plaster gets noticeably warm a few minutes after mixing and sets hard in 10–30 minutes. Set plaster rings faintly when tapped and cannot be dented with a thumbnail, though a fingernail can scratch it.
  • Weight check: 100 parts of gypsum should come out at about 84–85 parts of plaster. Much more means undercooked; much less (near 80) means overburnt.

Note Troubleshooting. Never sets, or stays soft and chalky → undercooked (still mostly gypsum) or dead-burnt (overheated). Cook a new batch: stop when the "boiling" stops, never let the pan glow. Sets in a minute or two, lumpy → water too warm, old set plaster in the bowl, or it was stirred too long. Use clean bowls and cool water; add a little glue to slow it. Sets but is weak and powdery → too much water, or it was re-stirred after it began to set. Use the island method. Plaster spoiled in storage → damp got in; re-cook it briefly. Bubbles and holes in casts → brush the first thin coat into the details, tap the mould, pour slowly from one side. Mould halves stuck together → not enough soap; soap three times next time. Wall plaster crumbles or blisters → the wall is damp. Use lime plaster there.

Dangers

Danger Never set a body part in a mass of plaster. Setting plaster gets hot. A small layer — a bandage cast — only gets warm, but a bucketful or a thick block can reach 50–70 °C and stay there for many minutes, causing deep burns that need amputation. People casting hands or feet in a bowl of plaster have lost fingers. Make body casts only with thin bandages over padding, and never put a hand into setting plaster.

  • Hot pans and steam. Cooking gypsum throws up hot dust and steam. Stir at arm's length and protect your eyes.
  • Dust. Plaster dust irritates eyes and lungs. Sift gently, outdoors, with a damp cloth over your nose and mouth. Rinse eyes with plenty of water.
  • Molten metal in damp moulds explodes into steam. Bake plaster moulds fully dry before pouring metal.
  • Collapsed gypsum ground. Because gypsum dissolves in water, gypsum country can hide caves and sinkholes that open without warning. Be careful digging or quarrying there (Quarrying and Cutting Stone).
  • Gypsum is not food. It has been used to adulterate flour; never mix it with anything people will eat, except as the specific food-grade use of curdling soy milk into tofu, which needs pure, clean gypsum.

What this unlocks

Plaster moulds lead to repeatable shapes everywhere: slip-cast Pottery, Stoneware and Porcelain and Laboratory Glassware supports, pressed Tiles and Clay Pipes, and lost-wax and sand casting in Metal Casting. Plaster walls and ceilings make homes clean and bright. Plaster casts and splints are a basic tool of Basic Surgery. And ground gypsum is the setting regulator that makes Portland Cement usable.

How it was first done

Gypsum plaster is one of humanity's oldest building materials: people in the Near East were heating gypsum and lime for plaster by about 9,000 years ago. The ancient Egyptians used gypsum mortar to set the casing stones of the Great Pyramid (about 2560 BC) and gypsum plaster for walls and painted surfaces. The name "plaster of Paris" comes from the huge gypsum quarries under Montmartre in Paris, worked since Roman times. After the Great Fire of London in 1666, the King of France ordered Paris's timber houses to be covered with plaster to protect them against fire, and the city's plaster became famous. In the 1760s the French chemist Antoine Lavoisier showed that setting is gypsum taking back the water lost in heating. The plaster bandage was invented in 1851–1852 by Antonius Mathijsen, a Dutch army surgeon, and used on a large scale by the Russian surgeon Nikolai Pirogov in the Crimean War.

Source: content/entries/earth/gypsum-and-plaster.md