Part 7 · Home and Daily Life
Games and Sports Equipment
How to make dice, playing cards, chess and draughts sets, board games and jigsaw puzzles; stitched leather balls, bladder footballs and rubber balls; cricket bats, bats and tennis rackets; nets and goals; ice skates, roller skates and sledges; medals and trophies — and how to lay out a level, true playing field.
- Difficulty
- ●●●●●
- Time
- An evening for a set of dice or draughts; a week for a chess set or a stitched football; a season for a level, drained playing field
- Steps from zero
- 7 prerequisites →
This unlocks
—The full path from nothing — 7 steps before this one
- Cordage and Rope
- Stone Tools
- Sulfur
- Hunting and Trapping
- Basic Woodworking
- Rubber
- Hides and Leather
- Games and Sports Equipment
Do them roughly in this order. See it on the tech tree →
Why it matters
Shared play holds a community together, lets young people test their strength without fighting, and keeps bodies fit. Board games and cards train memory, planning and arithmetic through long winter evenings, and dice gave the world its first ideas of chance, which became Statistics and Probability.
Most of this gear comes from skills you already have: Basic Woodworking and the The Lathe for pieces and bats, Hides and Leather and Sewing, Needles and Thread for balls, Rubber for bounce, Blacksmithing for skate blades, and Surveying and Levelling for a field.
How it works
Bounce. A ball hitting the ground squashes, storing energy like a spring, and springs back. Hair stuffing absorbs most of the blow; air under pressure in a bladder, or rubber, gives most of it back. More air makes a ball harder and livelier; less makes it kinder to feet and heads.
The sweet spot. A bat struck near its end or near the handle vibrates and stings. At one point, usually 15–20 cm from the toe, it does not. Leaving the wood thickest there (the spine of a cricket bat) puts the weight where the ball should meet it.
Fairness. A die lands on each face equally only if it is a true cube with its weight at the centre.
What you need
| Item | For | See |
|---|---|---|
| Cattle leg bone, boxwood or dense hardwood | Dice, draughts, chess pieces | Horn and Bone Working |
| Paper, flour paste, woodblocks or stencils | Cards, boards, puzzles | Paper, Printing |
| Vegetable-tanned cowhide 1.5–2 mm, waxed linen thread, awl | Balls | Hides and Leather, Sewing, Needles and Thread |
| Pig bladder or rubber sheet; cork; hemp or wool twine | Bladders and ball cores | Rubber |
| Willow, ash, hickory, rattan cane; gut string | Bats and rackets | Steam-Bending Wood |
| High-carbon steel strip | Skate blades | Steel |
| Netting twine, netting needle, gauge | Nets | Knitting, Crochet and Netting |
| Tin, pewter, copper or silver | Medals, trophies | Tin and Pewter |
| Lime, pegs, a long rope | Marking fields | Lime, Surveying and Levelling |
Where to find it
- Bat willow is the white willow of wet river meadows; the best grows fast and straight, with wide, even, pale rings. Any straight, clear willow makes a first bat.
- Ash grows on damp, rich soil, with diamond-patterned grey bark and black winter buds; its long grain bends without breaking. Hickory (eastern North America) is tougher still.
- Rattan is a climbing palm of South-East Asian forests with solid, springy cane stems. Without it, use laminated strips of ash.
- Bladders come from every pig or sheep butchered (Butchery and Meat); keep the neck long. Bone for dice and pieces is the straight shank of cattle, boiled clean (Horn and Bone Working).
Table games
Dice
- Saw a cattle shank bone or a bar of boxwood to a square section about 1.6 cm each side, and cut it into cubes.
- Rub each face flat on sandstone until every edge is the same length and opposite faces are parallel; check with calipers.
- Drill the pips 2 mm across and 1 mm deep. Opposite faces add to seven: 1 opposite 6, 2 opposite 5, 3 opposite 4.
- Fill the pips with soot in beeswax and polish.
Test. Roll each die 600 times: each face should come up about 100 times, and a face outside 80–120 suggests a biased die (roll another 600 to be sure). Or float it in salt water just strong enough to hold it up and spin it; a loaded die keeps turning the same face up.
Playing cards
- Card stock. Paste three sheets of paper together with thin flour paste (Glues and Adhesives), with soot in the middle layer's paste so the cards cannot be seen through. Press between boards under stones for a day.
- Print faces and backs from woodblocks or stencils (Printing, Screen Printing). Every back must be identical; any mark lets a player cheat.
- Cut to about 63 × 88 mm with a knife against a steel straight-edge, and round the corners to about 3 mm radius so they do not fray.
- Burnish both faces with a smooth stone, or wax and dust with talc, so they slide.
A pack is 52 cards: four suits of 13 (ace, 2–10, jack, queen, king), with the value printed small in two corners so a fanned hand can be read.
Chess and draughts
The board is 8 × 8 squares of 5–6 cm, alternately light and dark, with a light square in each player's right-hand corner. Paint it, or glue up alternate strips of pale and dark wood, cut across them, shift every other strip one square, and glue again.
Draughts (checkers): 12 pieces a side, discs 3–3.3 cm across and 7–8 mm thick sliced from a turned cylinder, half of them darkened.
Chess pieces, 16 a side, are turned on the The Lathe:
| Piece | Number | Height | Mark |
|---|---|---|---|
| King | 1 | 9–9.5 cm | A cross |
| Queen | 1 | 8–8.5 cm | A crown of points |
| Bishop | 2 | 7 cm | A mitre with a slanting cut |
| Knight | 2 | 6 cm | A carved horse's head |
| Rook | 2 | 5.5 cm | A notched castle top |
| Pawn | 8 | 5 cm | A small ball |
Make each base 40–50 % of the height across so it does not tip, and glue felt or leather underneath. Blacken one side with walnut-hull stain, or by brushing oak with vinegar in which iron nails have soaked for a week (Dyes and Mordants).
Other board games
Many fine games need only a board scratched on stone and some pebbles. Nine men's morris: three nested squares joined at their mid-sides, 24 points, 9 counters each; make a row of three to take a counter. Mancala: two rows of six cups carved in a board with a store at each end and 48 seeds; players sow seeds round the cups and capture, which drills counting. Backgammon: 24 long triangles, 15 counters each and two dice. Seal boards with linseed oil.
Jigsaw puzzle
- Paste a picture or map evenly onto a board 3–5 mm thick, and paste paper on the back too so it stays flat. Press overnight.
- Draw a wavy grid on the back, every piece with knobs and sockets that lock.
- Cut with a fret saw (a very fine blade in a deep bow frame; Files and Saws), the blade upright.
- Pieces of 2.5–4 cm suit adults; for small children cut a few pieces 8 cm or more from thicker board.
Balls
Leather ball
A soft handball: cut the cover as two figure-of-eight pieces or as four to six orange-peel segments, saddle-stitch them inside out (two needles through each hole), turn, and stuff very hard with animal hair, wool or sawdust.
A hard ball for cricket or rounders has a core:
- Pare a cork cube 2.5 cm across round, or use a small rubber ball.
- Wind wetted hemp or wool twine round it under strong tension, turning it constantly. Every few layers, hammer it round in a hemispherical hollow in hardwood. Stop just under the final size.
- Soak two or four cover pieces of 1.5 mm leather and stretch them over a wooden ball of the right size to dry hard in shape.
- Fit them over the core and sew with waxed linen thread pulled hard, leaving a raised seam.
- True the ball in two hemispherical cups squeezed in a vice; dye it with red ochre and polish with grease.
A cricket ball is 22.4–22.9 cm round and weighs 156–163 g.
Football
- Bladder. Rinse a fresh pig's bladder, rub it with oil, blow it up through a hollow reed and let it dry stretched. A bladder of cured rubber sheet with a long neck (Rubber) lasts far longer.
- Case. Cut 18 panels from a paper pattern, in six groups of three parallel strips, each group covering one face of an imaginary cube. Use hide 1.5–2 mm thick and cut every panel with the leather's stretch running the same way.
- Sew inside out with waxed thread, about 4 stitches per cm, leaving an 8 cm slit. Turn right side out.
- Fill. Push in the bladder, blow it up, tie the neck tightly and tuck it under the slit.
- Lace the slit with a criss-crossed thong over a leather tongue that protects the bladder, and grease the case with tallow.
A full-size football is 68–70 cm round and 410–450 g; dropped from 2 m onto hard ground it should bounce back 1.2–1.6 m. A rugby ball is made the same way from four long panels.
Rubber ball
- Solid. Press "soft rubber" mix (Rubber) into a two-part spherical mould, slightly overfilled, clamp and cure. It is nearly indestructible. Balls under 4.5 cm are a choking hazard (Toys).
- Hollow. Press two cups of rubber sheet over a hemispherical form, cement the edges together and cure; the trapped air keeps it firm. A tennis ball (6.5–6.9 cm across, 56–59 g) is a hollow rubber ball covered with two dumbbell-shaped pieces of Felt.
A good ball rolls straight, holds its air for days, and bounces the same whichever way it lands.
Bats and rackets
Bat
A round rounders or baseball bat is split (not sawn) from straight-grained ash or hickory so the grain runs its full length, then turned or shaved: 80–85 cm long, 6–7 cm at the barrel, 2.5 cm at the handle, with a knob at the end, about 0.9 kg. Grain running out at the handle means it will snap there.
Cricket bat
- Cleft. Split a willow log into wedge-shaped clefts, seal the ends with wax, and air-dry under cover for 9–12 months.
- Shape the blade: up to 96.5 cm long overall and 10.8 cm wide, the face flat, the back raised into a spine thickest (5–6 cm) about a third of the way up from the toe. Round the shoulders.
- Handle. Glue strips of rattan with thin strips of rubber or leather between them to absorb shock, and turn the bundle about 3.2 cm across and 30 cm long. Cut a V-shaped splice 12–15 cm deep into the top of the blade, shape the handle's end to fit, and glue it with hide glue.
- Bind the handle with glued twine and cover it with rubber or thin leather.
- Knock in. Willow is soft. Rub a few drops of raw linseed oil into the face, then beat the face and edges with a wooden mallet for 4–6 hours in total over several days, gently at first. Otherwise the first hard ball cracks it.
A good bat weighs 1.1–1.4 kg, has straight, even grain on the face, and rings when a ball is bounced on it.
Tennis racket
- Rip a knot-free strip of ash about 1.2 × 2 cm and 1.8 m long.
- Steam it about an hour per 2.5 cm of thickness (Steam-Bending Wood) and bend it at once round a form with an oval of pegs about 23 × 30 cm, bringing both ends together to make the throat and handle.
- Drive a shaped wedge across the throat and leave it on the form a week.
- Glue the ends between two wooden cheeks to make a handle about 3 cm across; wrap with leather.
- Drill slanting string holes every 1.5–2 cm round the head and round their edges.
- String with gut (Musical Instruments) or hard-twisted hemp: long strings first, then cross strings woven over and under, each pulled to about 20–25 kg.
The racket is about 68 cm long and 350–400 g. Keep it in a screwed wooden press, or damp warps the head.
Nets and goals
Knot nets with a netting needle and a gauge (a flat stick setting the mesh) using the netting knot (Knitting, Crochet and Netting), in tarred or oiled hemp twine 2–3 mm thick.
| Game | Item | Size |
|---|---|---|
| Tennis | Net | 0.914 m high at the centre, 1.07 m at the posts; mesh about 4 cm |
| Volleyball | Net | 9.5 m long, 1 m deep, top at 2.43 m (men) or 2.24 m (women); 10 cm mesh |
| Football | Goal | 7.32 m wide, 2.44 m high inside; posts no thicker than 12 cm; net mesh 10–12 cm |
Goal frames are two posts and a crossbar of 10–12 cm square timber, mortised and pegged (Doors, Windows and Joinery), either set 60–80 cm into the ground or built free-standing with a frame running back along the ground and pinned down with long iron stakes or sandbags.
Danger Unanchored goals fall on children. A free-standing goal is top-heavy, and children swinging on crossbars have pulled goals over and been crushed to death. Anchor every movable goal, every time, and let no one hang on one.
Wheels, blades and runners
Ice skates
Bone skates are the oldest: the long, straight foot bones of a horse or cow, ground flat on one face, drilled at each end and tied under the shoe with thongs. You glide on them, pushing with an iron-tipped pole in each hand.
Steel skates:
- Forge a strip of high-carbon steel (Steel) 25–30 cm long, about 2.5 cm tall and 3–4 mm thick, curled up at the front.
- File the bottom straight and square across, or very slightly curved along its length so it rocks a little.
- Rivet it into a groove in a hardwood stock the length of the foot.
- Harden, and temper to straw-blue.
- Strap the stock to the shoe at toe and heel, or screw it to a stout boot sole.
- Sharpen with a flat file drawn lengthwise, held square, until both edges are crisp. A sharp edge shaves a sliver from a fingernail.
Skate only on clear ice at least 10 cm thick for one person; see Snowshoes, Skis and Sledges for testing ice and rescue.
Roller skates
Fix two iron axles, 6–8 mm, in forged brackets under a hardwood foot plate 2 cm thick, one at the toe and one at the heel. Turn four wheels of boxwood 4–6 cm across and 2–3 cm wide, grease the axles with tallow, and strap the plate to the shoe. Later use iron wheels with leather or rubber tyres and Making Ball and Roller Bearings. Fixed axles go only straight; the rocking skate of 1863 mounted each pair of wheels on a truck that pivots on a slanted bolt against rubber pads, so leaning steers it.
Sledge
A play sledge is a small version of the hand sledge in Snowshoes, Skis and Sledges: two ash or oak runners 80–100 cm long and 10–15 cm high with curved fronts, three or four cross bars and a slatted seat, shod with iron strip. Keep it low; a low sledge rolls over less.
Medals and trophies
The simplest prize is a wreath of leaves. For something lasting:
- Cast medal. Carve the design in reverse in soapstone or slate, 4–5 cm across and 4 mm deep, with a pouring channel and a loop for a ribbon. Clamp a flat stone lid on and pour lead-free pewter or tin (Tin and Pewter, Metal Casting).
- Struck medal. Strike a disc of copper or silver between hardened steel dies cut in reverse. See Jewellery, Beads and Medals.
- Trophy. A cup turned in wood and oiled, cast in pewter, or raised from silver sheet over a stake (Sheet Metal and Rolling, Gold and Silver), with the winners' names engraved on the base year by year.
Laying out playing fields
- Choose well-drained, nearly level ground (drain wet ground first: Field Drains, Terraces and Erosion Control), long axis north–south so the low sun is not in players' eyes.
- Level it: remove stones, fill hollows, check with a straight-edge and water level (Surveying and Levelling). Leave a fall of about 1 in 100 so rain runs off.
- Sow a tough, short grass; mow and roll it often.
- Set out a corner with a rope loop knotted into 12 equal spaces, pegged into a triangle of 3, 4 and 5 spaces: the angle between the 3 and 4 sides is a right angle. Measure the sides, then check that both diagonals are equal.
- Mark lines 10–12 cm wide with whitewash (slaked Lime in water), brushed, poured from a slotted can, or rolled from a wheel running in a trough.
| Field | Size |
|---|---|
| Football | 90–120 × 45–90 m (100–110 × 64–75 m for full matches) |
| Cricket pitch (between the wickets) | 20.12 m (22 yards) × 3.05 m, rolled hard |
| Tennis court | 23.77 m long; 10.97 m wide (doubles), 8.23 m (singles) |
| Running track | 400 m inside lane: two 84.39 m straights, two half-circles of 36.5 m radius |
How to tell it worked
- Dice: every face 80–120 times in 600 rolls. Cards: no card can be told by its back, even against the light.
- Ball: rolls straight, bounces alike off every side, holds air a week.
- Bats: no sting from a well-hit ball; the cricket bat is uncracked after a hundred balls. Racket: strings tight and straight after an hour; head flat on a table.
- Skates: glide straight; the edge grips when you push sideways.
- Field: diagonals equal within a few centimetres; no puddles a day after rain.
Note Troubleshooting. Football soft overnight → loose neck tie or a pinhole; retie, or patch the bladder with rubber cement. Ball lopsided → panels cut with the stretch running different ways; recut. Cricket bat face cracks → not knocked in enough; oil lightly and knock in longer. Racket head warps → stored damp or out of its press; re-steam on the form. Skates slide sideways → edges rounded; file square. Cards stick together → paste not dry, or not burnished; dry, burnish, dust with talc.
Dangers
Danger Thin ice kills. Never skate or sledge on ice thinner than 10 cm, on moving water, or near reeds, outflows and springs. Go in groups, with a rope and a long pole on the bank. See Snowshoes, Skis and Sledges.
- Head injuries. A hard ball can kill if it hits the temple; batters and close fielders need padded caps and, later, helmets. A leather football soaks up rain and becomes much heavier; do not let children head a wet one.
- Skate blades cut; carry them in leather or split-wood guards.
- Sledge runs must not end in roads, water, trees, fences or rocks. One rider at a time.
- Gambling with dice and cards has ruined many households; a community may want rules about it.
What this unlocks
Dice and cards lead to Statistics and Probability. Leagues and their rules call for Organising a Community. Roller-skate wheels lead toward the The Bicycle. Toys for small children are in Toys, and climbing frames and play areas in Playgrounds and Outdoor Play.
How it was first done
Bone dice 4,500–5,000 years old have been found at Shahr-i Sokhta in Iran and in Indus Valley cities; Egyptians played senet by about 3000 BC, and the Royal Game of Ur dates from about 2500 BC. Chess grew from the Indian game chaturanga around the 6th century AD and spread through Persia to Europe. Playing cards appeared in China by the 9th century and reached Europe in the 1370s. The peoples of Mesoamerica played with solid rubber balls over 3,000 years ago, while Europeans kicked pig bladders in leather cases. Bone skates from northern Europe are thousands of years old, and the Dutch skated on iron blades set in wood by the 1400s. John Spilsbury of London made the first jigsaws, "dissected maps" for teaching geography, in the 1760s. Charles Goodyear's vulcanised rubber of the 1840s made bouncing balls cheap; James Plimpton patented the rocking roller skate in 1863, the year the Football Association wrote its first rules; and Walter Wingfield patented lawn tennis in 1874.
Source: content/entries/home/games-and-sport.md