◆ Rebuild

Part 3 · Metals

Anodising Aluminium and Titanium

Grow a hard, protective skin of oxide on aluminium by making it the positive pole in a bath of dilute sulfuric acid, then dye it any colour and seal it. Also hard anodising for wear, and colouring titanium by voltage alone; with the tanks, jigs and power supply to do it.

Difficulty
●●●●●
Time
A day to build a tank and jigs; about two hours from bare part to dyed and sealed; seconds to colour titanium
Steps from zero
30 prerequisites →

You need first

ElectroplatingAluminium

This unlocks

—
The full path from nothing — 30 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Salt
  13. Bricks
  14. Fermentation
  15. The Wheel and Axle
  16. Firebrick and Refractories
  17. Bellows
  18. Gears
  19. Copper Smelting
  20. Iron (the Bloomery)
  21. The Waterwheel
  22. Blacksmithing
  23. The Battery
  24. Magnets
  25. Electrolysis
  26. Copper Wire
  27. Electroplating
  28. The Generator
  29. The Electric Arc Furnace
  30. Aluminium
  31. Anodising Aluminium and Titanium

Do them roughly in this order. See it on the tech tree →

Why it matters

Bare aluminium protects itself with an oxide skin, but that skin is only a few millionths of a millimetre thick. It scratches, stains, goes chalky in salt air, and the soft metal beneath wears away fast. Anodising grows that skin a thousand times thicker by electricity — 5 to 25 µm for ordinary work, up to 100 µm for hard anodising — and makes it part of the metal, not a coat lying on top.

The result:

Titanium (Titanium) anodised in a mild bath grows a film so thin and clear that it shows colours by interference, like oil on water. The voltage alone sets the colour: bronze, purple, blue, gold, pink, green — with no dye at all. It colour-codes surgical implants and makes jewellery (Jewellery, Beads and Medals).

How it works

Anodising is Electroplating the wrong way round. The part hangs as the anode — joined to the positive (+) terminal. A sheet of lead or aluminium is the cathode (−). The bath is dilute sulfuric acid.

When current flows, oxygen is set free at the surface of the part, and it combines at once with the aluminium to make aluminium oxide (alumina, Al₂O₃, the same substance as sapphire and corundum). Hydrogen bubbles off the cathode.

The oxide does not conduct, so you might expect it to stop growing at once. But the acid slowly dissolves it at the same time. The two together produce a remarkable structure:

  • Right against the metal is a thin, solid barrier layer, about 1 nm thick for every volt — about 15 nm at 15 V.
  • Above it, the oxide grows as a honeycomb of tiny six-sided cells, each with a straight pore down its middle, 10–20 nm wide — about a five-thousandth of a hair. There are many billions to the square centimetre.
  • The current keeps flowing down the pores, so the coat keeps growing deeper into the metal. About two-thirds of the thickness grows inward, replacing metal; one-third builds outward. A part grows by about a third of the coat thickness on each face.

Dyeing fills the pores with colour. Sealing in hot water turns the oxide at the pore walls into a hydrated form (boehmite) that swells and closes the pores, locking the dye in and keeping dirt and salt out.

1 Anodisedpores open 2 Dyeddye soaks into pores 3 Sealedpore mouths swell shut pore 10–20 nmcellbarrier layeraluminium coat 5–25 µm thick, nearly as hard as corundumnot to scale: real pores are far narrower and closer together
Fig. 1 The anodic coat magnified. A barrier layer sits on the metal, with columns of oxide cells above it, each with a pore. Dye soaks into the pores; sealing in hot water swells the pore walls and closes them.

How thick. For ordinary sulfuric anodising, the thickness grows at about 0.3 µm per minute for every ampere per dm². At 1.5 A/dm² (amperes per square decimetre — a dm² is a 10 × 10 cm square) for 40 minutes, you get about 18 µm. Measure the area of the part and set the current from that, as for plating.

What you need

Item Notes See
DC power 0–24 V for ordinary work, up to 100 V for hard anodising and titanium; current 1.5 A per dm² of work Rectifiers: Turning AC into DC, Power Supplies and Regulators, The Rechargeable Battery, The Generator
Ammeter and voltmeter, or a copper coulometer Setting current density Measuring Electricity, Electroplating
Tank Glazed stoneware, glass, lead-lined wood, or acid-proof plastic; at least 4 litres of bath per ampere Stoneware and Porcelain, Lead
Cathodes Lead or pure aluminium sheet, about the same area as the work Lead, Aluminium
Jigs Aluminium or titanium wire and strip Below
Sulfuric acid Concentrated, about 1 litre per 10 litres of bath Sulfuric Acid
Cleaning Lye (sodium hydroxide), soda, nitric acid Lye and Potash, Soda Ash and Baking Soda, Nitric Acid
Cooling Lead or glass cooling coil with running cold water; ice and salt for hard anodising Ice and Refrigeration
Stirring Air bubbled from a pierced pipe along the bottom, from bellows or a pump Bellows to Air Compressors
Sealing pot Clean pot of distilled or rain water, kept near boiling Distillation
Dyes Alizarin from madder, weld, iron and cobalt salts, coal-tar dyes Dyes and Mordants, Coal Tar Chemicals

Where to find it

Everything is made in earlier chapters. Sulfuric acid comes from sulfur or pyrite (Sulfuric Acid); lye and soda from wood ash and natron (Lye and Potash, Soda Ash and Baking Soda). For dyes, madder root gives alizarin, which forms a brilliant red with aluminium oxide — the same chemistry as the alum-mordanted "Turkey red" of Dyes and Mordants. Weld gives yellow, and oak galls give tannin, which goes grey-black with iron salts.

Which aluminium. Pure aluminium and aluminium with a little magnesium, or magnesium and silicon, anodise clear and bright. Alloys with several percent of copper (strong aircraft alloys) or much silicon (most casting alloys) anodise grey and patchy, and burn easily. The fairly pure metal from your own cells (Aluminium) anodises well.

The anodising tank

DC supply 12–18 V − + − Thermometer air in Lead cathode negative (−) Hydrogen bubbles off Tank stoneware or lead-lined wood Air pipe bubbles stir the acid Part: the anode (+) 1.2–1.8 A per dm² Aluminium jig cold water in and out Cooling coil Acid bath 1 acid : 9 water 18–22 °C
Fig. 2 An anodising tank. The part hangs from the positive bar on an aluminium jig between two lead cathodes. Air bubbles stir the acid and a coil of cold water carries away the heat.
  1. Tank. For a first tank, a glazed stoneware crock or a big glass jar of 20–40 litres. For larger work, a wooden box of planks lined with sheet lead 3 mm thick, its seams burned (melted) together with a hydrogen flame or a soldering iron run hot (Soldering and Brazing). A lead lining can itself serve as the cathode.
  2. Bus bars. Two copper or aluminium bars across the top on wooden blocks: the middle one positive for the work, the outer ones negative for the cathodes. Keep them dry and clean; acid creeps up and corrodes contacts.
  3. Cathodes. Lead sheets hung on each side of the work, 10–15 cm away from it, giving about equal area to the work.
  4. Cooling. Anodising heats the bath. At 15 V and 10 A it makes 150 W, which warms 20 litres by about 6 °C an hour. Run cold water through a coil of lead pipe in the tank, or stand the tank in a larger tub of cold water.
  5. Agitation. Bubble air through a pierced lead or glass pipe along the bottom. This stirs the bath and sweeps hot acid away from the work. Never use oxygen.
  6. Thermometer hanging in the bath (The Thermometer).

Making up the bath

Fill the tank to three-quarters with clean water (rain or distilled). Then slowly pour in concentrated sulfuric acid, a thin stream, stirring, until you have added 1 volume of acid for every 9 volumes of water. This gives about 180–200 g of acid per litre (roughly 15–18% by weight). It gets hot; let it cool before use. Always acid into water, never water into acid.

The jig

Current must pass through a firm contact at every moment. The moment a loose contact grows oxide, the current stops and the part does not anodise.

  1. Make jigs of pure aluminium wire or strip (3–5 mm), or of titanium if you have it. Never use copper, brass or steel in the bath: they dissolve and spoil it.
  2. Grip each part tightly by springing it on, by a screw into a hole in an unseen place, or by twisting the wire hard around it. A spot where the jig touches stays bare; put it where it will not show.
  3. Hang parts so gas bubbles escape upward: no pockets or cups facing down.
  4. Aluminium jigs anodise too. Strip them in hot lye after every run so they make good contact again. Titanium jigs need stripping only when they lose contact.

Step by step: ordinary (sulfuric) anodising

  1. Finish the surface first. Anodising shows every scratch and file mark. Polish, brush or bead-blast the part to the finish you want before you start.
  2. Degrease in hot soap or soda solution, or wipe with spirit (Ether, Acetone and Solvents). Rinse.
  3. Etch in 5–10% lye at 50–60 °C for 30 seconds to 2 minutes. It fizzes and gives a clean, even satin surface. Longer etching makes it more matte. Rinse well.
  4. Desmut. The etch leaves a grey or black film of alloying metals. Dip in nitric acid, about 1 part acid to 2 parts water, for 30–60 seconds, until bright. Rinse. Test: water should spread evenly over the whole surface without breaking into drops (water-break test). If not, clean again.
  5. Anodise at once, without touching the part. Hang it on the positive bar, start at 0 V and raise the voltage over 1–2 minutes until the current reaches 1.2–1.8 A/dm². Expect about 12–18 V. Keep the bath at 18–22 °C. Fine bubbles rise from the cathodes; the part itself barely fizzes.
  6. Time it: 30–60 minutes for 10–25 µm. 40–45 minutes at 1.5 A/dm² is a good dyeable coat. The voltage creeps up slowly as the coat thickens.
  7. Rinse in two changes of clean cold water. Do not let it dry, and do not put it in hot water yet: heat begins sealing.
  8. Dye (below), or go straight to sealing for a clear finish.
  9. Seal. Hang the part in distilled or rain water at 96–100 °C for about 2–3 minutes for every micrometre of coat: 40–60 minutes for 20 µm. Or seal in water with 5 g per litre of nickel acetate at 85–95 °C for 15–20 minutes, which stops dye bleeding better. Tap water with lime in it leaves a powdery bloom.
  10. Dry and polish lightly with a soft cloth.

Dyeing

Dye straight after rinsing, while the pores are open.

  • Prepared dyes. Dissolve 1–5 g per litre of a water-soluble dye (Coal Tar Chemicals, Dyes and Mordants) in water at 50–60 °C, slightly acid. Dip for 5–20 minutes, checking the colour now and then by lifting it out. Deeper coats take darker colours.
  • Madder red. A strong, filtered extract of madder root (Dyes and Mordants) at 50–60 °C. The alizarin binds to the oxide as it does to an alum mordant: orange-red to deep red.
  • Weld yellow. Boiled weld, filtered, used warm.
  • Bronze to black, by two salts. Dip in cobalt acetate (50 g/L) for 2 minutes, rinse lightly, then in potassium permanganate (25 g/L) for 2 minutes (Potassium Permanganate). Repeat for darker shades.
  • Gold. Ferric ammonium oxalate, 10–25 g/L at 50–60 °C, gives a lightfast gold.

Natural dyes and many early coal-tar dyes fade in sunlight. Use them indoors; for outdoor parts use the mineral (metal salt) colours.

Hard anodising

For wear parts, not for colour.

Ordinary Hard
Acid 180–200 g/L 120–180 g/L
Temperature 18–22 °C −2 to +5 °C
Current 1.2–1.8 A/dm² 2.5–4 A/dm²
Voltage 12–18 V starts 20–25 V, rises to 50–100 V
Time 30–60 min 60–120 min
Coat 10–25 µm, clear 25–100 µm, grey to dark bronze
  1. Cool the bath with an ice-and-salt jacket or a refrigerating coil (Ice and Refrigeration), and stir hard with air. The heat at the surface is intense; without strong stirring the part burns — dark, powdery pits where current runs away.
  2. Bring the current up over 5 minutes. Hold the current steady and let the voltage rise as the coat thickens.
  3. Rinse. Hard coats are usually not sealed, because sealing softens them slightly. Seal only if corrosion matters more than wear.
  4. Allow for growth: a 50 µm coat adds about 25 µm per face. Machine parts that size undersize first.

Colouring titanium

Titanium's oxide does not grow into a porous coat. Instead, a thin, clear film grows until its thickness matches the voltage — about 2 nm per volt — and then the current almost stops. The film reflects light from its top and bottom surfaces, and the two reflections interfere, so a particular thickness shows a particular colour.

  1. Bath. 5–10% washing soda (Soda Ash and Baking Soda) or trisodium phosphate in water, or very dilute sulfuric acid (about 2%). Room temperature.
  2. Cathode. A strip of titanium or stainless steel.
  3. Clean. Rub the titanium bright with fine abrasive and wash it with soap and water. Do not touch the surface afterwards; fingerprints show as stains. (Industry etches with hydrofluoric acid first, for brighter colours; this is extremely dangerous and is not needed.)
  4. Anodise. Clip the part to the positive lead with titanium wire, dip it, and switch on at the chosen voltage. The colour sweeps through in a few seconds and stops changing when the current falls. Lift it out, rinse, dry.
Volts Colour
10–15 Bronze, light brown
about 20 Purple
25–30 Dark to bright blue
35–40 Light blue
45–50 Pale yellow
55–60 Gold
65–70 Rose, magenta
75–80 Violet
85–100 Blue-green, green

Colours vary with the bath and the alloy; make a test strip, stepping the voltage up by 5 V along it. Higher voltage is permanent: you can go up from blue to gold, but not back down without stripping the film. Pens, brushes and small sponges soaked in the bath and connected to the negative lead let you paint different colours on one piece ("brush anodising"). Niobium and tantalum colour the same way, more vividly.

How to tell it worked

  • Insulation. Touch two probes of a lamp-and-battery tester to the anodised surface: the lamp stays dark. Bare spots and jig marks light it.
  • Hardness. A sharp steel point drawn lightly across a good coat slides without leaving a bright line. A hard-anodised surface dulls a file.
  • Even colour. A good dyed part has the same colour everywhere, with only the small jig mark bare.
  • Seal test. Put a drop of ink or dye on the surface, wait a minute and wash it off with soap. A well-sealed coat cleans completely; an unsealed one keeps a stain.
  • Salt test. Leave a test strip half-dipped in salt water for a week beside an untreated strip. The anodised half should stay bright.

Note Troubleshooting. No coat, part stays bare → bad jig contact (tighten, strip the jig), or polarity reversed (the part must be positive). Dark burnt pits, part hot → current density too high, bath too warm, poor stirring, or a high-copper alloy. Lower the current, cool and stir. Coat soft and powdery → bath too warm (over about 25 °C) or run too long; or too much aluminium dissolved in an old bath. Patches without coat in hollows → gas trapped; rehang so bubbles escape. Dye will not take → coat too thin, or sealed by accident in hot rinse water. Anodise longer and rinse cold. Dye bleeds out or rubs off → poor seal. Seal longer, in clean, near-boiling water. White powdery bloom after sealing → hard tap water. Use rain or distilled water. Uneven, streaky colour → dirty surface; clean and desmut again; the water-break test must pass.

Looking after the bath. Top up with water as it evaporates and with acid as it is used. Each run dissolves some aluminium into it; when the bath anodises slowly and the coat gets soft, after a total of roughly 15–20 g of aluminium per litre has dissolved, make it up fresh.

Dangers

Danger Sulfuric and nitric acid. Strong acid blinds and burns deep. Wear eye protection, rubber or leather gloves and an apron. Always add acid to water, slowly, never water to acid: it can boil and spit. Keep a bucket of water and some soda nearby to wash spills. Nitric acid gives off choking brown fumes when it attacks metal; desmut outdoors or under a draught. See Sulfuric Acid and Nitric Acid.

Danger Electric shock. Hard anodising and titanium colouring use 50–100 V DC, enough to stop the heart when hands are wet with acid. Switch off before touching the work or the bars, keep one hand away from the tank, and stand on a dry board (Wiring and Electrical Safety).

  • Hydrogen comes off the cathodes. A spark at the bus bars can ignite it. Ventilate, and never make or break a live connection above the tank.
  • Lye etching baths burn skin and eyes (Lye and Potash).
  • Old recipes seal with potassium dichromate or anodise in chromic acid. Chromium(VI) compounds cause cancer and are not needed (Chromium and Its Compounds). Avoid them.
  • Hydrofluoric acid etches for titanium: never use it without proper training and a calcium antidote at hand.
  • Spent baths are acid with aluminium sulfate: neutralise with lime or soda before pouring away, never into a stream.

What this unlocks

Anodised aluminium makes light, durable kitchenware (Pots, Pans and Kettles), instrument and torch cases (Dry Cells and Electric Torches), window frames and roofs (Window Glass, Roofs), hydraulic and engine parts (Hydraulic Presses and Rams, The Internal Combustion Engine), and the skins and fittings of Gliders and Aeroplanes. The thin anodic film is also the insulator of the aluminium electrolytic capacitor (Resistors, Capacitors and Coils) that smooths every power supply. Coloured titanium serves jewellery and surgical implants (Crutches, Prosthetics and Rehabilitation).

How it was first done

That aluminium carries a current in only one direction in some baths was noticed in the 1850s and used in early electrolytic rectifiers. In 1923, Guy Bengough and J. M. Stuart in Britain patented anodising in chromic acid to protect seaplane parts from sea water. In the same years Japanese researchers at the Riken institute developed anodising in oxalic acid (sold as "Alumite"). Sulfuric acid anodising was patented in Britain by Gower and O'Brien in 1927, and dyeing and sealing the porous film followed in the late 1920s and 1930s. Hard anodising at low temperature was developed in the 1940s and 1950s for aircraft and military parts. Colouring titanium and niobium by voltage became popular with jewellers in the 1970s.

Source: content/entries/metals/anodising.md