◆ Rebuild

Part 3 · Metals

Iron (the Bloomery)

Smelt iron from bog ore or red rock in a clay chimney fed with charcoal and air. The result is a spongy "bloom" of iron and slag that you hammer into solid metal — the material of nearly every tool that followed.

Difficulty
●●●●●
Time
A week to build and dry the furnace; a full day per smelt, plus a day to consolidate the bloom
Steps from zero
10 prerequisites →

You need first

Finding and Identifying OresCharcoalBellowsFinding and Preparing Clay

This unlocks

Prussian Blue and the PrussiatesThe ElectromagnetMagnetsBlacksmithingThe Blast Furnace and Cast Iron

Objects made here

bloomery furnacebloomiron
The full path from nothing — 10 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)

Do them roughly in this order. See it on the tech tree →

Why it matters

Copper Smelting and Bronze are wonderful, but copper ore is scarce and tin is rare. Iron ore is almost everywhere: in bogs, red soils, black beach sand and rusty rock. Once people learned to smelt it, metal stopped being a luxury for chiefs and became something every farmer could own — axes to clear forest, ploughshares, sickles, nails, hinges, chains and cooking pots.

Iron is also the starting point for everything harder and stronger. Forged by a smith (see Blacksmithing) it becomes tools; given carbon, it becomes Steel, which takes an edge far sharper and harder than bronze ever could. With more heat and a water-powered blast, it becomes The Blast Furnace and Cast Iron. Iron is the metal of Magnets, of the The Steam Engine, of rails and machines. If this book has a single turning point between "surviving" and "industry", it is the first glowing bloom pulled out of a clay furnace.

It is also hard. Your first few smelts will probably give you nothing but slag. That is normal. Every iron-making people in history learned it by trial and error, and so will you — but with this chapter, much faster.

How it works

Iron melts at 1,538 °C — too hot for a simple charcoal furnace. The bloomery gets around this: it never melts the iron at all.

  1. Reduction. Charcoal at the bottom of a tall clay chimney burns in the air blast to carbon monoxide gas (CO). The hot CO rises through the charge of ore and charcoal and pulls oxygen out of the iron ore, turning it into tiny grains of solid metallic iron. This happens at about 800–1,100 °C, in the upper and middle part of the furnace.
  2. Slag formation. The ore also contains sand and clay (silica). At about 1,150–1,250 °C, near the air inlet, this silica combines with some of the iron oxide into a runny black glass called slag (mostly fayalite, an iron silicate). The slag melts, drips down, and washes the iron grains clean.
  3. The bloom. The iron grains, still solid but soft and sticky, weld together just below the air inlet into a spongy lump of iron soaked with slag: the bloom. The slag collects below it, and you drain it out through a hole in the base (tapping).

Two things follow. The ore must be rich, because the slag "eats" iron: an ore with too much sand turns entirely into slag and gives no iron. And the furnace must stay hot and choked with charcoal for hours, so that the gas stays full of CO and the slag stays liquid.

100–120 cmshaft height from the bellows Tuyeresloping 20–25° down 20–25 cm 25–30 cm inside Hearth pitcharcoal dust and ash Blue-tinged flamecarbon monoxide burning Charge1 kg charcoal, then 1 kg ore,each time the level drops Reduction zone800–1,100 °C: ore turns tograins of solid iron Clay wallclay + sand + straw, 10–15 cm Bloom grows here1,200–1,300 °C, yellow-white;slag melts and drips down Tap archclay plug; drain the slagevery 30–60 minutes Dry sand pittap slag cools black
Fig. 1 The bloomery furnace in cross-section. Charcoal and ore go in at the top; the blast enters through the tuyere; the bloom grows just below it and slag drains from the bottom.

What you need

Item Amount for one smelt Notes
Iron ore, roasted and crushed 15–25 kg Pea to hazelnut size (5–15 mm). See below and Finding and Identifying Ores.
Charcoal 40–60 kg 2–4 cm pieces, dry. About 20 kg for preheating, the rest for smelting. See Charcoal.
Clay mixed with sand and straw or dung 150–250 kg For the furnace. See Finding and Preparing Clay.
Bellows Two pairs, or one big double-action bellows 500–1,000 litres a minute. See Bellows.
Tuyeres 2–3 Fired clay, 2.5–3 cm bore. See Bellows.
Helpers 3–6 people Taking turns at the bellows over 6–8 hours.
Tools Long green-wood poles, a hooked iron or hardwood rake, wooden mallets, a big flat anvil stone, heavy hammerstones, a bucket to weigh charges

Where to find it

The best first ore is bog iron: rusty brown lumps and crusts from wet meadows and bogs, especially in sandy country. Look for orange water, orange slime and oily rainbow films on still water that break into plates when you poke them (oil films flow back together; iron films don't). Probe the bog with a sharpened pole; ore lies in a hard layer 10–50 cm down. Other good ores are red hematite, black magnetite and black sand. All are described in Finding and Identifying Ores.

Is it rich enough? Good ore is noticeably heavy. After roasting, it should be dark red to black, heavy, and mostly attracted to a lodestone. If your ore is light, sandy or full of visible quartz grains, look for better ore, or hand-pick and wash it; poor ore wastes a whole day.

Preparing the ore

  1. Dry it in the sun for a few days.
  2. Roast it in an open fire or heap until it glows dull red for 2–4 hours (see Finding and Identifying Ores). Roasting drives off water and carbon dioxide and makes the ore porous, so the furnace gases can get inside each lump.
  3. Crush the roasted ore with hammerstones on a flat stone to pieces 5–15 mm across — pea to hazelnut.
  4. Sieve out the dust through a coarse basket. Fine powder clogs the furnace and blows out of the top. Weigh the ore into equal charges of 1 kg (use a balance, see Measurement from Scratch, or just use a measured basket).

Building the furnace

A first furnace should be a simple shaft furnace (a clay chimney) built above a shallow pit:

Part Size
Inside diameter at the bottom 25–30 cm (about a forearm length across)
Inside diameter at the top 20–25 cm
Height of the shaft above the floor 100–120 cm (about waist to chest height)
Wall thickness 10–15 cm at the bottom, 6–8 cm at the top
Tuyere height above the floor 20–25 cm
Tuyere angle sloping down 20–25°, tip 3–5 cm inside the wall
Tap arch at the base 20 cm wide × 20 cm high, opposite or beside the tuyere
  1. Choose the site. Dry, level, well-drained ground, with a slight slope away from the tap arch, out of the wind, with a roof against rain if you can. Never on ground that floods.
  2. Dig the hearth. Dig a round pit 35 cm across and 15 cm deep where the furnace will stand. Fill it with charcoal dust mixed with ash and pack it down. This bed insulates the bottom and keeps the bloom from sticking to cold ground.
  3. Mix the clay. Use 1 part clay to 1 part coarse sand by volume, with plenty of chopped straw, dry grass or dung — enough that the mix holds together like stiff, hairy bread dough. The sand and fibre stop it cracking as it dries and heats.
  4. Build the base. Lay the clay in a ring around the pit, 10–15 cm thick, leaving the tap arch open (prop it with a stick frame or a stone lintel). Build up in rings or rolled coils, about 15–20 cm high per day, pressing each new layer firmly into the last. A woven wicker basket of the right size, set in the middle as a form, helps keep the shaft round; it burns out in the first fire.
  5. Fit the tuyere when the wall reaches about 20–25 cm above the floor. Push it through the wall sloping down at 20–25°, aimed at the centre, its tip 3–5 cm inside the wall. Seal clay round it.
  6. Finish the shaft to 100–120 cm high, tapering slightly. Smooth the outside. Leave a small hole (3 cm) in the tap arch plug for tapping slag, or plan to cut one.
  7. Dry it. Let it air-dry for 3–7 days, then light small wood fires inside for a day, building them up gradually. Cracks will appear; press fresh clay into them.

Step by step: the smelt

  1. Close the tap arch with a clay plug (clay mixed with sand), leaving the small tapping hole stopped with a lump of clay.
  2. Preheat (1–2 hours). Burn wood in the furnace, then fill it to the top with charcoal and blow gently. The walls must be thoroughly hot — glowing orange inside when you look down from the top — before any ore goes in. A cold furnace makes only slag.
  3. Set the rhythm. Bring the blast to full strength. The charcoal level will sink as it burns. Each time the level falls about 15–20 cm, add one charge: 1 kg of charcoal, then 1 kg of ore spread evenly on top. Start with half-ore charges (0.5 kg ore per 1 kg charcoal) for the first three or four, then go to equal weights.
  4. Keep time. In a 30 cm furnace with a good blast, a charge should go down every 10–15 minutes. Slower than 20 minutes means too little air: the furnace is too cool. Much faster than 8 minutes means too much: the ore has no time to reduce. Use a sand-glass or count bellows strokes and write each charge down.
  5. Watch and listen.
    • The furnace should roar steadily. Pulsing or wheezing means the blast is uneven.
    • Flames at the top should be lazy and yellow, with blue tongues; the blue is carbon monoxide burning — a sign the inside is reducing properly. A strong, pale blue-white flame is good.
    • Look through the gap at the back of the tuyere: the charcoal in front should be yellow-white, too bright to look at long. You may see dark drops of slag falling past.
    • If the tuyere starts to darken and the blast pushes back harder, slag is rising up to it.
  6. Tap the slag when it rises toward the tuyere — usually first after 1½–2 hours, then every 30–60 minutes. Push a long dry green stick or an iron rod through the tapping hole and wiggle it. Molten slag runs out orange-red, like slow lava, into a pit of dry sand in front of the arch. It cools to black, glassy, ropy cakes. Re-plug the hole with clay.
  7. Keep going for 4–6 hours of ore charging, putting in 15–25 kg of ore in total.
  8. Burn down. After the last ore, add one or two more charges of charcoal only, and keep blowing for 20–30 minutes so the last iron settles onto the bloom.

Extracting the bloom

Work fast — the bloom must be hammered while it is white-hot.

  1. Stop the blast, pull out the bellows nozzles, and break open the tap arch with a pole or stone.
  2. Rake out the glowing charcoal. Find the bloom: a heavy, lumpy, glowing mass usually stuck to the wall just below the tuyere. Prise it loose with a pole or iron bar and drag it out, or lift it out through the top with tongs.
  3. Knock off loose slag and charcoal and get it onto a flat stone or a big hardwood stump immediately.
  4. Compact it gently. A fresh bloom is crumbly. Hit it first with wooden mallets, or gentle hammerstone blows, all over, just to squeeze it together. Slag squirts out in sparks. Pieces that fall off — save them; they can be reforged.
  5. Reheat and compact. Once it starts to hold together, reheat it in a forge (see Blacksmithing) to a bright yellow to white heat (1,250 °C or more, when sparks begin to fly from the surface), and hammer harder. Repeat many times, squeezing out slag each heat.
  6. Cut, fold and bar. When it is solid, cut it in half with a hot chisel, stack the halves, heat them to welding heat and hammer them together. Then draw it out into a bar.
bright orange,straight from the furnace slag squirts out as sparks welding heat: white,sparkling surface faint slag lines stay 1 · Raw bloomspongy iron and slag 2 · Compactwooden mallets first 3 · Cut, stack, weldmany heats 4 · Bar ironready for the forge
Fig. 2 From bloom to bar. The raw bloom is spongy with slag; repeated heating and hammering squeezes the slag out and welds the iron solid.

Expect losses. A good smelt of 20 kg of rich ore gives a bloom of 3–5 kg. Consolidating it into clean bar iron loses a third to a half of that again. So a full day's smelt might give you 1.5–3 kg of usable iron — enough for several knives, an axe head, or a set of tools. A first smelt may give a few hundred grams, or nothing. Keep the bits; even small pieces can be welded together.

How to tell it worked

  • Weight. The bloom is much heavier than slag of the same size.
  • Lodestone. Iron grabs a lodestone strongly; slag barely or not at all.
  • The cut. Cut or file a corner. Iron shows a bright grey metallic surface; slag is black, glassy and shiny in a different way.
  • The bend test. Forge a small piece into a thin rod. Iron bends cold without breaking, and when it does finally break, it shows a fibrous, grey grain. Slag shatters.
  • Sparks. At white heat, the bloom spits bright sparks as you hammer it — that is iron burning, and a good sign.

Note Troubleshooting. Only slag, no bloom → ore too poor (too much sand), furnace not preheated, or not enough charcoal in the charges. Get richer ore, preheat longer, and try a lower ore-to-charcoal ratio. Slag froze and plugged the furnace → furnace too cold. More air, smaller charcoal, and tap the slag sooner so it does not drown the tuyere. Tuyere melted back and clogged → it was too far in, or the blast too strong. Set it with the tip just 3–5 cm inside, and keep spares. Bloom crumbles apart under the hammer → too cool when hammered, or hammered too hard at first. Use wood mallets first, at full heat. Bloom is very hard and cracks when forged → it picked up too much carbon (it is partly steel or even cast iron). Good! Sort these pieces out for Steel. Molten metal (not slag) ran out of the tap hole → the furnace was so hot and rich in charcoal that it made cast iron. Save it for The Blast Furnace and Cast Iron; next time, use a little less charcoal per charge.

Dangers

Danger Carbon monoxide. A bloomery is a carbon monoxide factory: the blue flame at the top is the gas burning. In a closed shelter, or downwind in still air, it can kill without warning. Smelt only in the open. Anyone with a headache, dizziness or confusion must leave the area at once.

Danger Molten slag and water. Slag at 1,200 °C hitting wet ground, a puddle or damp sand explodes into steam and flings burning droplets. The tapping pit must be filled with dry sand, and no water may be anywhere near the tap arch. Never smelt in the rain without a roof.

  • Burns. The furnace wall is hot enough to burn through clothes. Wear leather, wool or linen — never anything that melts. Stand to the side of the tap hole when tapping.
  • Flying sparks and slag. Compacting a bloom sprays white-hot slag. Everyone not hammering must stand back 3 m. Protect your eyes with a leather screen or squint behind a hand.
  • Collapse. An old, cracked furnace can fall apart while full. Check it before every smelt.
  • Exhaustion. Rotate bellows teams every 15–20 minutes, and drink plenty of water.

What this unlocks

The bloom becomes bar iron at the anvil: go next to Blacksmithing. Bar iron can be given carbon and hardened into Steel for edges, Springs and Files and Saws. A larger, taller furnace with a water-powered blast (see The Waterwheel) makes molten The Blast Furnace and Cast Iron that can be cast in moulds. Iron is also how you make Magnets and, with them, the The Compass.

How it was first done

People used iron from meteorites long before they could smelt it: beads in a grave at Gerzeh, Egypt (about 3,200 BC), and a dagger buried with the pharaoh Tutankhamun (about 1,325 BC) were both made of meteoric iron. Small amounts of smelted iron appear in Anatolia (modern Turkey) by about 2,000 BC, and after about 1,200 BC iron-working spread rapidly through the Near East, Europe and India — the start of what we call the Iron Age. Iron smelting was also developed in sub-Saharan Africa by around the 8th–6th centuries BC; whether it was invented there independently is still debated. Chinese metalworkers were making cast iron by the 5th century BC, far earlier than anyone else. In Scandinavia, Viking-age farmers smelted bog iron in small shaft furnaces very like the one in this chapter.

Source: content/entries/metals/iron.md