Shaping clay into pots by hand, drying them without cracks, and firing them in an open bonfire or a pit — giving you vessels to cook in, boil water, store food and carry liquids.

Difficulty
●●●●●
Time
An hour to shape a pot; one to three weeks to dry; half a day to fire
Steps from zero
2 prerequisites →

You need first

Finding and Preparing ClayFire

This unlocks

DistillationDyes and MordantsFermentationLye and PotashBottles, Drinking Glasses and GlasswareGlazesThe Potter's WheelSaltTar, Pitch and GlueTiles and Clay PipesBiogas and Wood GasGranaries and Food StorageCutlery and TablewareKitchen and CookingLamps and CandlesCopper SmeltingMercury
The full path from nothing — 2 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery

Do them roughly in this order. See it on the tech tree →

Why it matters

A fireproof pot changes how people live. With one you can boil — and boiling is how you make Finding and Purifying Water safe, cook grains and beans, render fat, extract dyes and medicines, and make soup that feeds the sick, the old and babies. Pots keep grain and seed dry and safe from mice. They hold water in camp. They ferment beer and vinegar (Fermentation), carry fire from place to place, and boil down seawater for Salt.

Pottery is also your first step into controlled high heat. The same lessons — dry slowly, heat slowly, cool slowly — lead straight to the The Kiln, Bricks, Lime, Glass, and the crucibles and furnace linings of Copper Smelting and Iron (the Bloomery) smelting. Chemistry needs pots too: Lye and Potash, Soap, Distillation and Dyes and Mordants all begin in a clay vessel.

This chapter covers shaping pots by hand and firing them in an open fire — methods that need no structure at all, and that people used for at least 15,000 years. Enclosed, hotter firing is in The Kiln.

How it works

Fired clay is artificial stone. As you heat a dry pot:

Temperature What happens What you see
Up to 100 °C Leftover water in the pores evaporates Steam; pot feels damp-warm
100–200 °C Trapped water boils out Danger stage — wet pots burst
200–500 °C Roots, straw and dung inside burn away Pot turns grey or black, then lighter
450–700 °C Water locked inside the clay crystals is driven off — the change to ceramic Dull red glow in the dark
573 °C Quartz grains in the clay suddenly change size slightly Cracks if heated or cooled too fast here
600–900 °C The clay hardens and strengthens Dull to cherry red glow

An open fire can reach 600–900 °C for a short time. That makes earthenware — hard, porous pottery that rings when struck and never turns back to mud. Fired at the low end it is weak and soaks up water; fired at the high end it is stronger.

What you need

Item Amount Notes
Prepared, wedged clay with temper 1–2 kg per medium pot See Finding and Preparing Clay. For cooking pots, 25–35% sand or grog
A smooth board, flat stone or mat 1 To work on; a broken pot base turned upside down makes a turntable
Smoothing tools A few A shell, a piece of gourd, a smooth wooden rib, a flat stick
A smooth pebble 1 For burnishing — the size of an egg, glassy-smooth
A wooden paddle and a round stone 1 each For the paddle-and-anvil method
Cord or thin blade 1 For cutting clay
Fuel for firing See below Dry wood (any), bark slabs, dried dung cakes, dry grass, sawdust
Water and a cloth To keep hands and clay damp

For a bonfire firing of 5–10 medium pots you need roughly a large armful of kindling and 2–4 large armfuls of split dry wood (wrist-thick), or a similar pile of dried dung cakes.

Shaping pots

Three methods cover almost everything. Whichever you use, follow these rules:

  • Even walls. Keep walls the same thickness everywhere — about 6–10 mm, a little thicker than a pencil. Thick and thin parts dry and heat at different speeds, and crack where they meet. A thick base is the most common fault.
  • Round shapes. Rounded bottoms and smooth curves survive heat far better than sharp corners. Cooking pots especially should have round bottoms; they sit in the embers and spread the heat.
  • Small first. Your first pots should be no bigger than two fists. Make many. Most first pots fail; that is how you learn.
  • Keep it damp while working. Cover finished parts with a damp cloth or leaves.
thumb fingers turn after each squeeze 6–8 mmeven wall new coilthumb-thick scrapedsmooth smeareach join score + slipevery edge slabs 8–10 mm thick PINCHcups, small bowls, crucibles COILany size, cooking and storage pots SLABboxes, trays, tiles, moulds
Fig. 1 The three hand-building methods. Pinch: press a thumb into a ball and squeeze the wall thin while turning. Coil: stack ropes of clay and smear them together. Slab: join flat sheets of clay along scored and slipped edges.

Pinch pots

The simplest method, good for cups, small bowls, lamps and crucibles.

  1. Roll a ball of clay the size of an orange (about 8 cm across).
  2. Push your thumb straight down into the centre until it is about 1 cm from the bottom.
  3. Squeeze the wall gently between thumb (inside) and fingers (outside), starting at the bottom. Turn the ball a little after each squeeze. Work upwards in a spiral.
  4. Go round three or four times, thinning a little each time, until the wall is 6–8 mm thick. Smooth the rim with a wet finger.

Coil pots

The most useful method: pots of any size, from cups to storage jars as tall as a child. Most traditional pottery in the world is coil-built.

  1. Make a base. Flatten a ball into a disc 1 cm thick and as wide as you want the bottom of the pot. Or press clay into a shallow dish or a hollow in sand to make a rounded base.
  2. Roll coils. On a damp board, roll clay under your spread fingers into ropes as thick as your thumb (about 1.5 cm) and 30–50 cm long. Keep them covered.
  3. Score and slip. Wherever two pieces of clay join, score both surfaces — scratch criss-cross lines with a stick — and brush on slip (clay mixed with water to a thick cream). Joins made without this crack apart in drying.
  4. Lay the coils. Lay a coil round the edge of the base, pinch off the excess, and join the ends. Lay the next coil on top. Each coil sits a little inside the last to bring the wall in, or a little outside to swell it out.
  5. Smear the joins. After every two or three coils, smear clay from each coil down onto the one below with a thumb or finger — on the inside and the outside. A coil pot whose coils are not smeared together will split along them.
  6. Rest. After 4–6 coils, stop for 15–30 minutes and let the wall stiffen a little, so it can carry the weight of more clay without slumping.
  7. Scrape and thin. Scrape the walls with the edge of a shell or a gourd piece, inside and out, to even them out and thin them to 6–10 mm. Rotate the pot as you work.
  8. Paddle and anvil (optional but excellent). Hold a smooth round stone inside the pot against the wall, and pat the outside opposite it with a flat wooden paddle. This thins, compacts and strengthens the wall, and closes hidden cracks. Work round the pot in rows.

Slab pots

Good for flat-sided boxes, trays, tiles, lamps and moulds.

  1. Flatten clay on a cloth into a sheet 8–10 mm thick. Two sticks of that thickness laid either side, with a round stick rolled across them, give an even slab.
  2. Let the slabs stiffen until they bend without sagging (an hour or two).
  3. Cut the pieces you need. Score and slip every edge, press them together, and run a thin coil of clay along each inside joint, smearing it in.

Finishing

  • Rims. Smooth and slightly round every rim with a wet finger or a piece of wet leather. Rims dry fastest and crack first.
  • Burnishing. When the pot is leather-hard — firm, cool and damp, like stiff leather, so a fingernail marks it but it does not bend — rub the surface hard with a smooth pebble, in small overlapping strokes. The clay surface packs down and begins to shine. Burnished pots are stronger, smoother, and soak up less water. Burnish again when nearly dry for a high gloss.
  • Decoration and handles. Press patterns with a cord, a shell or a stick while the clay is still soft. Add handles and lugs by scoring and slipping, as for coils.

Drying

Drying is where most pots are lost. The secret is slow and even.

  1. First days (1–3): covered. Keep the pot in shade, out of wind and sun, loosely covered with a cloth or leaves. Wrap the rim and any handles in a damp strip of cloth so they do not dry ahead of the body.
  2. Then (1–2 weeks): uncovered, in shade. Turn the pot upside down when the rim is firm, so the base can dry. Turn it every day.
  3. Last days: in warmth. Put it in the sun, or near (not beside) a fire.

A pot is bone dry when it has turned paler all over and evenly, when it no longer feels cool when held against your cheek, and when it rings faintly when flicked. If any part still feels cool, it still holds water. Small pots take about a week; large thick ones take three weeks or more. In humid or cold weather everything takes longer.

Warning Never fire a pot that is not bone dry. Water left inside turns to steam and blows the pot apart, often throwing hot fragments and wrecking the pots next to it.

Method 1: Open bonfire firing

The oldest method, still used by potters in Africa, Asia and the Americas. It reaches about 600–850 °C.

OPEN BONFIRE PIT FIRING Fuel all roundno pot showing Keep feedinguntil pots glow red Pots mouth-downpre-heated first Bed of emberson dried ground Big fire on top2–3 hours sherds or bark fine fuel packedround and inside pots mouth-up sawdust or dung 40–60 cm 1–3 hours · about 600–850 °C · cool slowly under the ashes then cover with earth and leave overnight
Fig. 2 Open bonfire and pit firing in cross-section. In both, pots are first warmed to drive out the last water, then completely surrounded by fuel so they heat evenly.
  1. Choose a site. Flat, bare, dry ground, sheltered from wind, at least 5 m from anything that can burn. Wind is the enemy: it heats one side and chills the other, and cracks pots.
  2. Dry the ground. Burn a fire on the firing spot for an hour to drive water out of the soil. Rake the embers to the side.
  3. Pre-heat the pots ("water smoking"). Set the pots in a ring about 50 cm from a modest fire, mouths facing the flames. Every 10–15 minutes turn them a quarter turn and move them a little closer. After 1–2 hours they should be too hot to hold with a bare hand for more than a moment (well over 100 °C). Steam that has been rising from them stops. This step is what prevents most blow-ups.
  4. Set the pots. Spread a bed of embers and dry kindling 5–10 cm deep on the hot ground. Stand the hot pots on it, mouth-down or on their sides, close together but not touching. Put small pots inside or beside big ones.
  5. Build the fuel around them. Lean dry sticks and bark slabs upright all round the pile like a teepee, until no pot can be seen. Fill gaps with dry dung cakes and grass. Use plenty of fuel: the pots must be completely surrounded.
  6. Light it all round at once, so it burns evenly.
  7. Keep it covered. As the fuel burns down, the pots will show through. Lean more fuel against any bare spot. Keep the fire going for 1–3 hours. Look in when the flames die back: the pots should be glowing dull red to cherry red, evenly all over.
  8. Let it cool slowly. When you stop feeding it, rake the ashes and embers over the pots and leave them. Do not remove them until you can pick them up barehanded — usually several hours, best overnight. A hot pot taken into cold air, or splashed, cracks with a sharp tink (called dunting).

Method 2: Pit firing

A pit holds heat better than a bonfire, shelters pots from wind, and cools them slowly. Pots usually come out dark, smoky black or patchy — beautiful, and just as useful.

  1. Dig a pit 40–60 cm deep and wide enough to leave 15 cm of space around the pots. Burn a fire in it for an hour to dry and warm it, and rake out the embers.
  2. Pre-heat the pots beside the fire, as in step 3 above.
  3. Bed: put 10 cm of fine fuel in the bottom — sawdust, crumbled dry dung, wood shavings, dry leaves.
  4. Pack: set the pots in, mouth up, and fill around and inside them with more fine fuel, then small sticks and broken dung cakes, up to ground level.
  5. Cover with large pieces of broken pottery or slabs of bark to slow the burn, and build a large fire on top of the pit. Keep it going 2–3 hours.
  6. Seal the pit by letting the fire burn down, then shovelling a layer of earth over the embers. Leave it overnight, or a full day, before digging the pots out.

How to tell it worked

  • Sound. Tap the pot with a knuckle or stick. A well-fired, sound pot rings with a clear, bell-like note. A dull thunk means a hidden crack, or underfiring.
  • Colour. Fired clay is red, orange, buff, brown, grey or black. Black and grey patches ("fire clouds") are where fuel touched the pot and are harmless. A dark grey core with a lighter skin, seen in a broken piece, means the inside never got hot enough to burn clean — fire longer next time.
  • The soak test. Leave a broken piece (or the pot) in water overnight. If it softens or a fingernail scrapes off mud, it was not hot enough (below about 550 °C) — refire it.
  • The scratch test. A fingernail should not scratch a good earthenware pot.
  • The water test. Fill it with water. Earthenware is porous, so the outside will turn damp and "sweat" — that is normal. It should not drip.

Note Troubleshooting. Pot burst into pieces, with fresh-looking clay inside → not dry enough, or pre-heated too quickly; dry longer and water-smoke for longer. Pieces blown out of the surface like craters → air bubbles (wedge better) or lumps of lime (white specks — see Finding and Preparing Clay). Long straight crack after firing → cooled too fast or in wind; cover with ashes and wait. S-shaped crack across the base → base thicker than the walls, or not compacted; press the base firmly when making it. Crumbles, stains your wet finger → underfired; refire hotter with more fuel. Cracks along the coils → coils not smeared together; score, slip and smear.

Sealing pots

Earthenware is porous. That is useful in a water jar — water seeping to the surface evaporates and keeps the contents cool — but bad for storing oil, milk or honey, and wasteful in a cooking pot. Ways to seal it:

  • Use it. Simply cooking porridge or stew in a new pot seals it gradually: starch and fat fill the pores.
  • Milk or starch seal. Fill the new pot with milk, or with the cloudy water from boiling grain, and simmer it for half an hour. Pour it out and let the pot dry. Repeat two or three times.
  • Bark-tea seal. Many African potters splash or dip their pots, while still hot from the firing, in a strong brew of boiled tree bark or pods rich in tannin (oak, acacia, pine bark and many others work). It leaves a dark, water-resistant, glossy skin.
  • Resin or wax. For pots that hold liquids but are not heated, warm the pot by the fire and rub the inside with pine resin or beeswax, which melts into the pores. (Do not cook in these — the coating softens.)
  • Burnishing before firing, as above, reduces porosity a great deal.
  • Glaze — a glassy skin fused onto the pot — is the permanent answer. See Glazes.

Dangers

Danger Bursting pots throw hot fragments. A pot with water trapped inside can explode in the fire, throwing pieces several metres. Stand back during the first half hour of firing, keep children well away, and never lean over the fire to look.

  • Burns. Fired pots stay dangerously hot for hours, and fired clay looks the same hot or cold. Handle with thick leather or wet cloth, or wait.
  • Thermal shock. Never put an empty clay pot over a flame or pour cold water into a hot pot — it can crack and spill boiling contents. Heat cooking pots gently at first, with liquid in them.
  • Fire spread. Bonfire and pit firings throw sparks. Clear the ground, fire on a calm day, and keep water and loose earth ready (see Fire).
  • Lead. Never use old lead-glazed pottery from ruins for cooking or storing acid foods: lead leaches out and poisons slowly.

Going further

How it was first done

The oldest known pots were made at Xianrendong Cave in southern China about 20,000 years ago, and in Japan (by the Jōmon people) about 16,000 years ago — by hunter-gatherers, long before farming. Pottery was invented again, separately, in North Africa around 10,000 years ago and in South America around 7,000 years ago. All of these pots were hand-built and fired in open fires, as described here. Enclosed kilns appear in the Near East by about 6000 BC, and the potter's wheel in Mesopotamia between about 4500 and 3500 BC. Even today, millions of pots a year are coil-built and bonfire-fired in villages across Africa and South Asia.

Source: content/entries/earth/pottery.md