◆ Rebuild

Part 8 · Chemistry

Lampblack and Carbon Black

The blackest, finest powder there is, caught from smoky flames. Lampblack from oil, tar and resin makes ink and paint; channel and furnace black, made by the tonne from gas and oil, make tyres last many times longer and batteries conduct. Pressed with pitch and baked, carbon becomes the rods of arc lamps and batteries and the brushes that carry current into every motor and generator.

Difficulty
●●●●●
Time
An afternoon to build a lampblack collector; a week to run a soot house; two weeks to press and bake carbons and brushes
Steps from zero
5 prerequisites →

You need first

Lamps and CandlesCharcoal

This unlocks

—
The full path from nothing — 5 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. Charcoal
  5. Lamps and Candles
  6. Lampblack and Carbon Black

Do them roughly in this order. See it on the tech tree →

Why it matters

A gram of good lampblack is made of grains ten thousand times smaller than a grain of sand, with a surface of tens of square metres. That fineness is the secret of its uses:

  • Ink and paint. The deepest, most permanent black. It does not fade in sunlight or dissolve in water once bound (Ink, Pigments, Paints and Varnish, Printing).
  • Rubber. Mixed into rubber, carbon black multiplies the wear life of a tyre several times and protects it from sunlight. Without it the The Motor Vehicle would need new tyres every few hundred kilometres (Rubber).
  • Batteries. Fine carbon threads current through the poorly conducting powders of dry cells and lead–acid plates (Dry Cells and Electric Torches, The Rechargeable Battery).
  • Electrodes and brushes. Pressed and baked, carbon makes the rods of arc lamps and cells and the sliding contacts of motors and generators.

This chapter scales up the lampblack of the Ink chapter, outlines the industrial blacks, and turns carbon into electrical parts.

How it works

When oil, fat, resin or gas burns with too little air, part of the fuel is torn apart by heat without burning, and its carbon atoms join into tiny spheres clustered in short chains: soot. Soot that reaches the hot edge of the flame burns away; soot carried out and cooled first survives.

Two rules follow:

  1. Starve the flame of air and you get more soot.
  2. Cool it quickly and the grains stay small. Small grains are blacker, stronger in ink and paint, and reinforce rubber better.
Kind Made by Grain size Yield from fuel Best for
Lampblack Oil, tar or resin burning smokily in a closed space 60–200 nm (coarse for a black) Roughly 10–25% Ink, paint, polish, batteries, electrodes
Channel black Many small gas flames touching cool iron channels 10–30 nm (finest) 2–5% Best inks, paints, carbon paper
Furnace black Oil sprayed into a very hot furnace, then quenched with water 15–80 nm, chosen at will 40–65% Tyres and rubber; most carbon black today
Thermal black Natural gas cracked by hot bricks with no air 150–500 nm (coarse) About 40% Soft rubber, plastics
Acetylene black Acetylene gas split by its own heat 30–50 nm, very pure Most of its carbon Dry batteries: conducts best

(A nanometre, nm, is a millionth of a millimetre.)

Graphite is carbon whose atoms are arranged in flat, slippery sheets. It conducts electricity well, lubricates, and resists heat. Ordinary soot and baked carbon are disordered; heated above about 2,500 °C they rearrange into graphite.

What you need

Item Use
Clay oil lamps with thick wicks, or a shallow iron pan Burners
Plant oil, animal fat, pine resin, pine tar, coal tar or heavy crude oil Fuel (Oils and Pressing, Tar, Pitch and Glue, Petroleum and Refining)
Clay or iron bowls; bricks and lime mortar; coarse cloth or sacking Collectors and soot house (Bricks)
Feathers, soft brushes, tin scoop, lidded clay pots Collecting and calcining
Coke, retort carbon or charcoal; coal-tar pitch Electrodes and brushes (Coal and Coke, Coal Tar Chemicals)
Natural graphite Brushes, better electrodes
Steel die and screw or lever press; iron tube Shaping carbons (Presses, Punches and Dies)
Kiln or brick box, coke dust Baking (The Kiln)

Where to find it

  • Fuels for lampblack: heavy, smoky oils: seed oils, fish oil, tallow, pine resin and pine tar, coal tar and heavy crude oil. Alcohol and good kerosene burn too cleanly.
  • Natural gas for channel and thermal black seeps from the ground in oil regions and over coal seams (Natural Gas and Helium).
  • Graphite occurs as grey, greasy, metallic flakes and lumps in schist, gneiss and marble, and where coal seams have been baked by volcanic rock (Pencils and Chalk).
  • Retort carbon, the hard grey crust that grows inside gasworks retorts (Coal and Coke), is dense, pure and conducts well, the best raw material for arc lamp and battery carbons.

Method 1: Lampblack collectors

The bowl collector

This is the Ink chapter's plate held over a lamp, multiplied.

  1. Set 6–10 clay oil lamps in a row along a bench, each with a thick wick of twisted cotton or flax pulled out until the flame is 4–6 cm tall and smoking.
  2. Over each, hang an inverted clay or iron bowl 15–20 cm across, on a frame, with its inside surface 3–5 cm above the flame tip. The flame should just lick it. Unglazed fired clay holds soot well.
  3. Screen the row from draughts; a steady flame makes even, fine soot.
  4. Every 20–30 minutes, swap each bowl for a cool one and brush the soot into a lidded pot with a feather. A bowl that gets too hot burns its soot grey.

Expect 2–5 g an hour per lamp: enough for ink and small paint jobs, not for rubber.

The soot house

Firing chamber Flue 15–20 cm square Sacking catches soot chambers about 1 m each way Chimney damper Air door nearly shut Pan of resin, tar or oil smoky, lazy flame Coarse soot near the fire Finest soot in the last chamber
Fig. 1 A soot house. Resin, tar or heavy oil burns in a shallow pan in a small firing chamber with a nearly closed air door. The smoke flows through a chain of chambers hung with sacking; soot settles on every surface, coarse near the fire and finest in the last chamber, before the cooled gas leaves by the chimney.

For kilograms, burn fuel in a closed chamber and let the smoke settle in a chain of rooms, as Chinese and European black-makers did for centuries.

  1. Firing chamber. Build a brick box about 60 × 60 × 60 cm with a small iron door at the bottom front that can be opened 1–2 cm to let in air. Inside, on a brick hearth, stand a shallow iron pan 30–40 cm across.
  2. Settling chambers. From the top of the firing chamber, run a flue 15–20 cm square into a line of three or four brick or clay-plastered wooden chambers, each about 1 m on a side, joined by openings at alternate top and bottom corners so the smoke must zig-zag. Hang sheets of coarse sacking or cloth from the ceilings. Fit each chamber with a tight door.
  3. Chimney. From the last chamber, a short chimney with a damper sets the draught. Too much draught burns the soot; too little puts the fire out.
  4. Burn. Put 2–3 kg of resin, tar or heavy oil in the pan and light it. Close the air door until the flame is lazy, dark orange and pouring out thick black smoke. Keep feeding fuel. One charge lasts several hours.
  5. Collect. After a day or two of burning, let everything cool for at least 12 hours, then shake the sacking and sweep the walls into lidded tubs. Keep the chambers apart: the first gives coarse, greasy soot for rubber and tar paints; the last the finest black for ink.

Expect roughly 1 kg of lampblack from 5–10 kg of fuel.

Cleaning and calcining

Raw lampblack holds oily tar that stops it mixing with water and slows oil paint. Pack it in a clay crucible with a clay-sealed lid and heat it to a dull red (about 700 °C) for an hour; let it cool unopened. This calcined lampblack is blacker and wets easily.

Method 2: The industrial blacks, in outline

Channel black. Hundreds of small, flat gas flames, each about 5 cm long, touch the undersides of iron channels that slide slowly back and forth; fixed scrapers sweep the soot into hoppers. It is the finest black of all, but only 2–5% of the gas becomes soot, and the waste and smoke ended it.

Furnace black. Heavy oil is sprayed into a blast of burning gas in a brick-lined furnace at 1,400–1,800 °C. It cracks into soot in a few thousandths of a second; a water spray a metre or two on quenches it, and cloth bag filters catch it. The temperature and the distance to the spray set the grain size. The fluffy black is rolled with water into beads so that it pours without dust.

Thermal black. Two towers of firebrick take turns: one is heated red-hot by burning gas while natural gas, with no air, is passed through the other and splits into hydrogen and coarse soot.

Acetylene black. Acetylene (Calcium Carbide and Acetylene) splits into carbon and hydrogen by its own heat once started in a closed vessel, giving the best-conducting black. Acetylene can decompose explosively under pressure: this is a works process only.

Using carbon black

  • Ink: calcined lampblack ground with gum for writing ink; raw lampblack in linseed varnish for printing ink, at about 1 part black to 4–6 parts varnish (Ink, Printing).
  • Paint: lampblack has a cool, slightly bluish tone. It is so strong that a pinch greys a pot of white. In oil it dries slowly: add a drier or a little Prussian blue (Prussian Blue and the Prussiates). Mixed with lime it makes grey limewash (Lime).
  • Rubber: mill 40–60 parts of carbon black into 100 parts of rubber for tyre treads, 20–40 for shoe soles and belts, adding it a little at a time on the mill until no grey streaks remain (Rubber). Synthetic rubbers need it even more: SBR tyre rubber is weak and useless without it (Synthetic Rubber Works (Overview)). The rubber comes out black, tough, and far more resistant to wear and sunlight. A modern tyre is about a quarter to a third carbon black by weight.
  • Batteries: a few per cent of acetylene black or fine lampblack in the manganese dioxide bobbin of a dry cell carries current through it (Dry Cells and Electric Torches); a pinch in the negative paste of a lead–acid plate keeps it spongy (The Rechargeable Battery).
  • Other uses: shoe and stove blacking (lampblack in wax and turpentine), matt black inside cameras and telescopes (Photography, The Telescope), carbon paper (Envelopes, Stamps, Clips and Office Supplies), and black plastics, which it shields from sunlight (Petrochemicals and Modern Plastics).

Method 3: Carbon electrodes

The basic process of pressing coke and pitch and baking it is in The Electric Arc Furnace (large furnace electrodes) and The Light Bulb (arc lamp rods). This section adds what makes small, fine, dense carbons for lamps, cells and laboratory work.

Fine-grain carbons

  1. Raw materials. Grind calcined coke or retort carbon to flour that passes fine cloth. Use 60 parts of this, 15 parts calcined lampblack, and if you have it up to 10 parts natural graphite flour.
  2. Bind. Knead in about 25 parts of coal-tar pitch, melted at 150 °C, until every grain is coated and the mass is like stiff, warm clay. Fine powders need more binder than coarse ones.
  3. Extrude. Pack the warm paste into a steel cylinder and force it out through a die (a hard steel plate with a smooth, slightly flared hole) with a screw press. Hole sizes: 6–10 mm for battery rods, 10–20 mm for arc lamp carbons and small electrolysis anodes. Cut the emerging rod to length on a board and keep it straight.
  4. Cored carbons. For arc lamps, fix a thin steel pin in the centre of the die so the rod comes out as a tube with a 2–3 mm hole. After baking, fill the hole with a paste of soft graphite flour and water glass (Water Glass (Sodium Silicate)) and bake again. The soft core holds the arc steady in the middle of the rod.
  5. Bake packed in coke dust in a sealed box, rising no more than 10–20 °C an hour to about 1,100 °C (orange-yellow), holding a few hours, then cooling slowly. The cycle takes a week.
  6. Densify. Soak the baked rods in hot pitch (better under a vacuum, The Vacuum Pump), and bake again. Two rounds make a dense, strong rod.
  7. Finish for cells. Boil battery rods in melted paraffin wax for 10 minutes. The wax fills the pores so the cell's liquid cannot creep up the rod and corrode the brass cap.

Graphite electrodes (outline)

Baked carbons become graphite at 2,500–3,000 °C. In Acheson's furnace, baked rods are laid crosswise in a long brick trough, packed in coke granules and buried under sand and coke dust. Heavy current, fed through carbon blocks at the ends, heats the pile white-hot for several days; it cools for a week or more. Graphitised electrodes carry three times the current of baked ones and last far longer as anodes in chlorine and magnesium cells (Chlorine and Bleach, Magnesium); soak them in linseed oil to close their pores.

Testing electrodes

  • A good rod rings when tapped, is uniformly dark grey when broken, with no cracks, soft centre or layers.
  • Density: about 1.5–1.7 g per cubic centimetre for baked carbon (weigh it, then measure its volume by the water it displaces).
  • Resistance: a 10 cm length of 10 mm baked rod should measure about 0.05–0.07 Ω end to end; graphitised, about a fifth of that (Measuring Electricity). Twice the expected figure means too little baking or a cracked rod.

Method 4: Carbon brushes

Spring presses 150–250 g on each cm² Brass box holder 0.1–0.2 mm play round the brush Carbon brush spans 2–3 segments Copper pigtail many fine strands Terminal Gap 2–3 mm holder to commutator Commutator copper segments with mica between rotation The brush cut open Tamped joint copper powder rammed hard round the wire Curved face bedded to the commutator
Fig. 2 A carbon brush and its holder. The brush, a small block of baked carbon or graphite, slides in a brass box holder a few millimetres above the commutator. A spring presses it down. Current leaves through a flexible copper pigtail fixed into a hole in the top of the brush with packed copper powder.

Copper strip or wire brushes (The Electric Motor, The Generator) groove the commutator and spark badly on big machines. Carbon lubricates itself, wears instead of the copper, and its slightly higher contact resistance damps the spark as each commutator segment leaves the brush.

Grades

Grade Made from Current per cm² of contact Use
Carbon-graphite Coke, lampblack, some graphite; baked 6–8 A Slow DC generators and motors
Electrographite Carbon-graphite brushes graphitised 10–12 A Most industrial motors, traction motors
Natural graphite Flake graphite with a little binder 8–10 A Small fast motors, slip rings
Metal-graphite 40–90% fine copper powder with graphite 15–25 A Low-voltage, high-current machines: plating dynamos, battery chargers, car starters, slip rings

Making carbon-graphite brushes

  1. Mix 50 parts fine coke flour, 20 parts calcined lampblack and 10 parts graphite flour, with about 20 parts of hot pitch. Knead, let it cool and harden, then crush it to coarse granules: this moulding powder packs evenly.
  2. Press blocks. Fill a steel die with the powder, warmed, and squeeze it hard with a screw press: as much pressure as you can get, ideally a tonne or more on each square centimetre. Press blocks about 25 × 50 mm across and 50 mm deep: pressing the 12.5 cm² face takes 12 tonnes or more. More pressure means a denser, stronger brush.
  3. Bake them packed in coke dust as for electrodes, to about 1,100 °C, slowly. Graphitise some if you can (above).
  4. Cut and grind. Saw blocks into brushes with a fine saw or abrasive wheel (Abrasives and Grinding Stones). Grind all four sides flat and square on a plate with fine emery, then wash off all emery dust: it is conductive and abrasive and will ruin the commutator.
  5. Size. Brush contact area per brush arm = current ÷ current density. A 40 A carbon-graphite arm needs about 5–6 cm², for example two brushes of 12 × 25 mm. A brush should span about two to three commutator segments.
  6. Fit the pigtail. Drill a hole 3–4 mm across and 8–10 mm deep in the top. Push in the end of a flexible stranded copper lead (many fine wires, Copper Wire), then pack fine copper powder around it in small doses, ramming each dose hard with a punch. This tamped joint grips tightly and carries the full current. A copper rivet through a slot also works.

Metal-graphite brushes: mix fine copper powder (from Electroplating or copper sulfate reduced with iron) with graphite and a little pitch, press as above, and heat packed in charcoal to 700–850 °C, well below the melting point of copper.

Holders and springs

  • A box holder is a brass or bronze sleeve the brush slides in, with 0.1–0.2 mm play in thickness and a little more in width. Too tight and the brush sticks; too loose and it chatters.
  • Set the bottom edge of the holder 2–3 mm above the commutator.
  • A spring (a coiled steel clock spring or a lever spring, Springs) presses on the top of the brush with 150–250 grams for each square centimetre of contact, or up to twice that on machines that shake, such as tram motors.

Bedding in

New brushes must be shaped to the commutator's curve. Wrap a strip of glass paper (sand glued to paper, not emery) around the commutator, sand side out, and pull it back and forth under each brush, or in the direction of rotation only, until the whole face is curved and grey. Finish with fine paper, blow out every grain of dust, then run the machine lightly loaded for some hours.

Good and bad brushes

  • Good: a glossy face over the whole area, barely visible sparking, and a thin, even, chocolate-brown skin on the commutator. Never clean this skin off; it is what makes carbon brushes work.
  • Bad: streaky or bare copper, grooves, chattering, heat-discoloured pigtails, or a ring of sparks. Check spring pressure, grade, holder play and the commutator's roundness.

A brush wears a few millimetres per thousand running hours. Replace it when it is down to about a third of its new length.

How to tell it worked

  • Lampblack: a pinch rubbed on white paper with a fingertip gives a deep, even black, not brown or grey. Calcined black stirred into water with a drop of gum disperses at once; raw black floats in clumps.
  • In rubber: a cut through milled rubber is uniformly black with no grey streaks or specks.
  • Carbons and brushes: see the tests above.

Note Troubleshooting. Little soot, flame burns clean → too much air. Close the air door or shorten the wick. Soot grey or brown, with red sparks in it → the collector or chamber got too hot and the soot burned. Use cooler bowls, a longer flue, or less draught. Greasy, lumpy soot → raw tar in it. Calcine it. Rods crack in the bake → heated too fast, or paste too wet with binder. Slow the first 500 °C. Rods soft and crumbly → too little binder or pressure, or air reached the bake. Brushes spark and the commutator blackens in patches → poor bedding, wrong spring pressure, or a rough commutator. Re-bed and check the springs.

Dangers

Danger Soot houses catch fire, and a chamber full of fine soot can flash when opened hot. Let every chamber cool for at least 12 hours before opening, keep lamps and pipes away from the doors, and never sweep with a light nearby. Build the soot house apart from other buildings.

  • Carbon monoxide. A starved flame makes it in quantity. Run soot houses and lamp rows outdoors or in open sheds, never in living rooms (Chimneys, Stoves and Heating).
  • Breathing soot. Fine carbon black and tar fumes harm the lungs, and long exposure to the tarry soot of coal and oil causes cancer; chimney sweeps' cancer was the first known industrial cancer. Wear a damp cloth mask when sweeping, wash well after work, and keep children out.
  • Pitch fumes from baking electrodes are also harmful. Bake outdoors or with a good chimney (Tar, Pitch and Glue).
  • Graphitising furnaces carry huge currents at 3,000 °C: for an established electrical works only (Wiring and Electrical Safety).

What this unlocks

How it was first done

Soot ink was in use in ancient Egypt by about 3000 BC and in China by the second millennium BC. Chinese ink-makers burned pine wood and later tung and sesame oil in long brick kilns and lamp rooms and graded the soot by how far it had travelled. In Europe, Kienruß from pine resin was probably a German trade by the 1600s.

Channel black was first made from natural gas in the United States in the 1870s. In 1904 S. C. Mote in Britain found that carbon black greatly strengthens rubber, and from about 1912 tyre makers adopted it; tyres turned from white to black. Oil furnace black came in the 1940s and replaced channel black for most uses.

Carbon electrodes began with Humphry Davy's arc of about 1808, using charcoal; Robert Bunsen made pressed coke electrodes for his battery in 1841. Charles Van Depoele introduced carbon brushes for motors in 1888, and Edward Acheson, while making silicon carbide, found graphite in his furnace and patented artificial graphite in 1896.

Source: content/entries/chemistry/carbon-black.md