◆ Rebuild

Part 6 · Building

Cob, Adobe and Rammed Earth

How to build strong, warm, lasting walls from the ground under your feet — choosing the right soil, then building it up as cob, laying it as adobe blocks, ramming it between boards, or plastering it onto woven sticks — and how to keep it dry so it stands for centuries.

Difficulty
●●●●●
Time
A few weeks for a small room with a team of three or four; a full season for a house
Steps from zero
1 prerequisite →

You need first

Finding and Preparing Clay

This unlocks

Insulation and Keeping Buildings Warm or Cool
The full path from nothing — 1 step before this one
  1. Finding and Preparing Clay
  2. Cob, Adobe and Rammed Earth

Do them roughly in this order. See it on the tech tree →

Why it matters

The soil under your feet is the cheapest building material on Earth. It needs no fire and no fuel, only digging. Earth walls are fireproof, quiet, and so heavy that they soak up the day's heat and give it back at night — an earth house is cool in summer and slow to chill in winter. Built well, they last: cob farmhouses in England over 500 years old are still lived in, and adobe towns in America, Africa and Arabia are older still.

This chapter turns the wattle-and-daub hut of Shelter and the mud brick of Bricks into real houses with thick walls. It covers choosing the soil, four ways to build, and — most important — keeping the walls dry. With Lime you will render them; with timber you will roof them (Roofs) and frame them (Timber Framing and Log Building).

How it works

Every soil is a mix of four parts, sorted by grain size:

Part Grain size Feels like Job in a wall
Gravel Over 2 mm Little stones Skeleton: carries load, never shrinks
Sand 0.06–2 mm Gritty Fills gaps, stops cracking
Silt Finer than sand Smooth, like flour Filler; weak, washes out easily
Clay Finest Sticky and slippery when wet The glue

Clay is the only part that sticks, but it also swells when wet and shrinks as it dries, so pure clay cracks to pieces. Earth building is a balance: enough clay to bind, enough sand and gravel to stop shrinkage, and — for cob and adobe — straw, which ties the mass together the way steel bars tie concrete, so cracks cannot spread (see Finding and Preparing Clay).

The second rule: dry earth is strong; wet earth is mud. A dry cob wall carries a two-storey house. The same wall soaked from below or from rain running down its face softens and slumps. Earth walls do not die of old age; they die because water got in. Every detail of a good earth building — the stone base, the wide roof, the lime render — keeps water out while letting the wall breathe out the dampness it does pick up.

Choosing the soil

Never use topsoil. The dark, crumbly top 20–40 cm is full of roots and rotting matter and never hardens. Scrape it off and keep it for the garden (Understanding Soil). Build with the subsoil beneath it: firmer, rootless, usually yellow, brown, orange or red.

The jar test

  1. Fill a straight-sided clear jar or bottle (Glass) one-third with broken-up subsoil, stones over 2 cm removed. Top up with water and add a pinch of salt (it helps clay settle).
  2. Shake hard for two minutes and stand it still.
  3. Gravel and sand settle within a minute — mark the top. Silt settles over an hour or two — mark it. Clay settles over a day or more as the water clears.
  4. Compare each layer with the total height.

No jar yet? Stir soil into lots of water in a clay-lined trench, let it settle and dry, and read the layers in a cut through it.

THE JAR TEST Waterclears slowly Claysettles in 1–2 days Siltsettles in 1–2 hours Sand and gravelsettle in 1 minute One-third soil, the rest water and a pinch of salt. Shake, then wait. ROUGH TARGETS Cob Adobe Rammed earth 15–25% clay, plus lots of straw 15–30% clay, plus some straw 8–18% clay, gravelly, no straw claysiltsand + gravel
Fig. 1 The jar test, and what mix suits each method. Sand settles first, then silt; clay settles last and slowly. Measure the layers and compare them with the targets.
Method Clay Silt Sand and gravel Fibre
Cob 15–25% Under 20% 55–75%, with some fine gravel Lots of straw
Adobe 15–30% Under 30% Mostly sand Some straw or dung
Rammed earth 8–18% Under 30% 50–75%, plenty of gravel up to 2 cm None
Daub (on wattle) 25–40% Any The rest sand Straw, hay or dung

Too much clay → bad cracks: add sand. Too little → crumbles: add fatter clay dug elsewhere. Too much silt → weak and easily washed: add sand and clay, and protect the wall well.

Always make test samples. Make three blocks about 25 × 12 × 8 cm of each mix and dry them two weeks in shade. Good ones have no big cracks, you cannot snap a corner off with your fingers, and a block dropped flat from waist height onto hard ground does not shatter. Change one thing at a time and write down each result.

What you need

Item For a room 4 × 5 m, walls 2.4 m high Notes
Building subsoil 25–35 m³ (50–70 tonnes) for cob or rammed walls 45 cm thick Dig on site if you can; moving it is most of the work
Sand Up to a third of the soil volume Only if the soil is too clayey
Straw About 1–2% of the soil's weight Long, dry, unrotted grain straw or tough dry grass. Not for rammed earth
Water Hundreds of litres A pond, stream or rain pit nearby
Stone for the plinth 6–10 m³ Field stone or quarried stone (Stone Masonry)
Timber Lintels, a ring beam, the roof Timber Framing and Log Building, Roofs
Tools Spades, a mattock, baskets, a big tarp or old hide, a rammer, a plumb line Wooden spades shod with iron last far longer

Method 1: Cob

Cob is wet earth and straw, mixed into a stiff dough and built up by hand, with no forms and no bricks. It is the easiest method to learn.

Mixing

  1. Soak. Heap the subsoil, make a hollow in the top, fill it with water and leave it overnight.
  2. Tread. Mix with bare feet, twisting on your heels — or let cattle do it. On a tarp or hide, two people roll the mix over by lifting one edge, tread it flat, and roll again.
  3. Add straw a handful at a time, treading it in. Long straw, 20–30 cm, ties the wall best.
  4. Judge it. Good cob is like very stiff dough: a squeezed ball holds its shape and oozes no water. Tear a lump apart and straw should bristle from both faces. Sloppy → add dry soil. Cracks when squeezed → add water.

Building

Tread it downtwist the heels to stitch layers Fresh liftlumps pressed into the last spade: pare it when leather-hard Firming liftwait 2–7 days between lifts Dry liftstraw ties it together Stone plinthtop 45 cm or more above ground Stitching stick 30–50 cmper lift 45–60 cm thick
Fig. 2 Building a cob wall. Each lift is 30–50 cm high, trodden onto the one below, then left to firm up. The faces are pared straight when leather-hard.
  1. Start on the plinth — never on the ground. The stone plinth is as wide as the wall, its top at least 45 cm above ground.
  2. Lay the first lift. Press fist-sized to head-sized lumps onto the plinth, each into the last. Walls are 45–60 cm thick for one storey, 60–90 cm for two.
  3. Tread it down from on top of the wall, and stitch each new layer into the old by working it down with a stick or heel so the straw reaches across the join.
  4. Stop at 30–50 cm. A wet lift that is too tall bulges and slumps. Wait until it takes a thumbprint only with effort — 2–7 days.
  5. Pare the faces straight with a sharp spade held flat while the lift is leather-hard. Check with a plumb line (Measurement from Scratch). A slight inward lean as the wall rises, a few cm per metre, is good.
  6. Openings. Build in wooden frames or lintels (beams over openings), resting at least 30 cm into the wall each side. Keep every opening at least 1 m from a corner.
  7. Cover the wall top every night and whenever rain threatens.
  8. Finish with a ring beam: a continuous timber (or two poles joined by crosspieces) bedded along the top of every wall and joined at the corners. It spreads the roof's weight and ties the walls together — the one detail that saves most earth houses in earthquakes.

Four people can raise a few cubic metres of cob a day. Thick walls take months to a year to dry right through; render only when dry.

Method 2: Adobe

Adobe is sun-dried mud brick (making it: Bricks). The slow drying happens on the ground in thousands of separate bricks, so the wall goes up fast.

  1. Mortar of the same soil, sieved, no straw, joints 1–2 cm. Never use mortar harder than the bricks.
  2. Lay the bricks dry — adobe softens if dipped.
  3. Bond them like fired Bricks: each vertical joint over the middle of a brick below, with a crosswise course at least every third course in thick walls.
  4. Corners first, plumbed and levelled, then a string line for each course. About 1 m of height a day at most.
  5. Thickness 30–45 cm. Keep unbraced height under 8 times the thickness (a 40 cm wall no taller than 3.2 m), and brace long walls with cross-walls every 4–5 m.
  6. Lintels and ring beam exactly as for cob.

Method 3: Rammed earth

Rammed earth (pisé) is damp — not wet — earth pounded in thin layers between strong boards until it is like soft stone. It needs no straw and dries in weeks, but needs more equipment and muscle. It makes the hardest, handsomest earth walls.

Rope tietwisted tight with a stick Poststops the boards spreading Spacer stickremoved as the earth rises Loose layer10–15 cm of damp earth Rammed layerseach squeezed to two-thirds Putlogcross-piece carrying the form Finished courseforms stripped at once Rammer5–9 kg head,1.5 m handle Upright post Side boardplanks 3–4 cm thick,60–90 cm high 30–50 cm lift 30–40 cm
Fig. 3 Rammed earth formwork. Two strong boards are held apart by cross-pieces below and pulled together at the top. Damp earth goes in 10–15 cm at a time and is rammed until it rings.

Formwork. Two side panels 60–90 cm high and 2–3 m long, of planks 3–4 cm thick nailed or pegged to battens so they cannot bend — a bulging form makes a bulging wall. Short stout putlogs laid across the wall carry the boards; upright posts outside the boards stand on the putlog ends, and their tops are pulled together with a rope twisted tight by a stick. Spacer sticks the width of the wall keep the boards apart until the earth reaches them. An end board closes the box.

Rammer. A wooden or stone head of 5–9 kg with a flat face 10–15 cm across, on a 1.5 m handle.

  1. Mix the soil damp. Sieve out stones over 2–3 cm. Add water a little at a time, turning it, until evenly damp — only 8–12% water by weight. It feels cool, never sticky.
  2. Drop test. Squeeze a handful hard into a ball (if it won't hold, it is too dry). Drop it from shoulder height onto hard ground: shatters into a few pieces → right; flattens or stays whole → too wet; turns to dust → too dry.
  3. Fill 10–15 cm of loose earth into the form — no deeper.
  4. Ram the edges first, then the middle, lifting 30–40 cm and letting it fall hard, overlapping blows. The layer shrinks to about two-thirds.
  5. Listen. At first each blow thuds and leaves a deep print. When the layer is done, the rammer bounces and rings and leaves almost no mark. Then add the next layer.
  6. Strip and move. When the form is full, take it apart at once and move it along. Step the end of each block so the next one keys into it, and stagger the joints of each course above like bricks. Fill putlog holes with earth afterward.
  7. Walls are 30–50 cm thick; ram lintels in over openings and finish with a ring beam.

Tip Stabilising. In wet climates, mix 5–8% slaked lime by volume (Lime) into a clayey soil and ram it within a few hours; the wall resists water far better. Later, a little Portland Cement does the same for sandy soils.

Method 4: Wattle and daub

Woven sticks plastered with clay — the method in Shelter — is the lightest way to fill a timber frame (Timber Framing and Log Building). Cut a groove under each beam and drill holes in the top of the beam below; spring upright hazel or oak staves into them every 30–40 cm, weave withies between, and daub both sides at once with 1 clayey earth : 1 sand plus plenty of straw or fresh cow dung. Panels are 10–15 cm thick. Fill the cracks after a week.

Plaster and render

  • Earth plaster (inside, or sheltered outside): sieved clayey soil with 2–3 parts fine sand and chopped straw, 1–2 cm thick on a dampened wall, polished with a flat stone when leather-hard.
  • Lime render (outside): the three coats in Lime, about 20–25 mm in all. First roughen the wall — scratch or peck it, or press small stones and pot shards into the face — so the render can grip. Keep each coat damp for a week.
  • Limewash: 3–5 thin coats, renewed every year or two. The cheapest weatherproofing there is.

Warning Never seal an earth wall with something waterproof — cement render, tar, oil paint. Water always gets in somewhere, usually from below; a waterproof skin stops it getting out, and the earth behind turns to mud unseen until the wall falls. Lime and earth "breathe". This is how modern repairs most often destroy old earth houses.

Keeping the wall dry

Builders say an earth wall needs "good boots and a good hat."

Good hatwide roof throws rain clear Ring beamties the wall tops together Earth wallcob, adobe or rammed earth Damp-proof layerslate, tar or birch bark 45 cmor more Good bootsstone footing and plinth,down to firm subsoil Gravel drainground slopes away Lime render Sill drip 50–60 cm+ rain splashesup from the ground
Fig. 4 An earth wall that will last. The stone plinth keeps its feet out of splash and ground damp; the roof overhang keeps rain off its face; a ring beam ties it together; lime render and drainage do the rest.
  • Good boots. A stone or fired-brick footing down to firm subsoil (Foundations and Floors), carried up as a plinth at least 45 cm above ground — rain splashes about that high. Lay a damp-proof layer on top of the plinth if you can (slates, tar, or birch bark: see Foundations and Floors).
  • A good hat. Eaves overhanging 50–60 cm or more, deeper on the side facing the rainy wind (Roofs).
  • Drainage. Slope the ground away from the walls, at least 5 cm fall in the first 1.5 m, and dig a gravel ditch on the uphill side. Never pile earth, firewood or compost against the wall.
  • Sills that stick out and slope outward, so rain drips clear.
  • Look after it. Fill cracks and limewash every year or two; inspect the foot of every wall after each wet season.

How to tell it worked

  • A dry cob or adobe wall sounds solid when struck with a fist and does not dent under a hard-pressed thumbnail.
  • Rammed earth shows clean layers like sedimentary rock and you cannot scrape grains off with a fingernail.
  • A sharp stick pushed into the wall goes in only with effort and leaves a clean hole.
  • After heavy rain, the foot of the wall is dry, with no damp stain creeping up from the plinth.
  • The house stays cool on hot afternoons and holds warmth through cold nights.

Note Troubleshooting. Deep cracks in cob or adobe → too much clay or water. Add sand and straw; build drier and slower. A cob lift bulges → too wet or too tall. Cut out the bulge; wait longer between lifts. Rammed earth crumbles at faces or corners → too dry, layers too thick, or under-rammed. Use the drop test; ram until it rings. Rammed layers separate → the top of the last layer dried out. Scratch and dampen it before adding more. Render falls off in sheets → wall too smooth or dry, or render too hard. Roughen, dampen, use lime. The base of a wall crumbles → plinth too low, ground sloping inward, or a hard render trapping water. Fix the cause, cut out soft earth and patch with fresh cob.

Dangers

Danger Earth walls can collapse without warning. A wet wall, a wall undercut at its base, or a wall shaken by an earthquake can fall all at once — a metre of wall weighs over a tonne. Unreinforced earth houses kill many people in earthquakes. In earthquake country keep walls thick and low, keep openings small and away from corners, brace long walls with cross-walls, tie the wall tops with a continuous ring beam, and prefer a light roof (Building Against Earthquakes and Storms).

  • Formwork can burst or topple; never stand on a form that is not firmly tied.
  • Rammers crush toes and fingers. Use steady, controlled blows.
  • Soil pits cave in and later fill with water and drown children. Slope their sides and fence them.
  • Strain. You will move tonnes of soil. Share the work, lift with your legs, and use barrows (The Wheel and Axle).
  • Kissing bugs. In Central and South America, insects carrying Chagas disease hide in cracks in mud walls and thatch. Smooth plaster, filled cracks and regular limewash remove their hiding places (Infectious Diseases).
  • Lime burns skin and eyes — see Lime.

Going further

How it was first done

The first farming villages of the Near East, over 10,000 years ago, built with packed mud and hand-made mud bricks; at Jericho the bricks still carry their makers' thumbprints. In China, rammed earth (hangtu) was used for town walls more than 4,000 years ago, and much of the early Great Wall in the dry northwest is rammed earth. The Roman writer Pliny the Elder described walls in Spain and North Africa "packed in between two boards" that had stood for centuries. Taos Pueblo in New Mexico has been lived in for about a thousand years. In Yemen, Shibam is a walled town of mud-brick tower houses five to eleven storeys high, mostly rebuilt over the last few centuries on far older foundations. And in Devon, England, thousands of cob farmhouses built from the 1400s onward still stand.

Source: content/entries/building/earth-building.md