◆ Rebuild

Part 14 · Electronics and Computing

Semiconductors and the Transistor

Some crystals let electricity through in one direction only, and a pinch of the right impurity changes how well they conduct by a factor of thousands. From the cat's-whisker radio detector to the copper-oxide rectifier and the transistor — the tiny switch and amplifier that replaced the vacuum tube.

Difficulty
●●●●●
Time
An afternoon for a crystal detector; a week for copper-oxide rectifiers; months to years, with a team, for the first transistors
Steps from zero
42 prerequisites →

You need first

The Vacuum TubePure Silicon

This unlocks

Germanium, Gallium and Compound SemiconductorsIntegrated CircuitsLight-Emitting DiodesHall Sensors and MagnetometersPhotocells and SensorsPower Electronics and Motor DrivesPower Supplies and RegulatorsSolar CellsLasers
The full path from nothing — 42 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. The Kiln
  10. Pottery
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Bricks
  15. Salt
  16. Mercury
  17. Lye and Potash
  18. Fermentation
  19. The Wheel and Axle
  20. Glass
  21. Firebrick and Refractories
  22. Bellows
  23. Saltpeter
  24. The Lathe
  25. Gears
  26. Copper Smelting
  27. Iron (the Bloomery)
  28. Laboratory Glassware
  29. Sulfuric Acid
  30. Pumps
  31. The Waterwheel
  32. Blacksmithing
  33. Hydrochloric Acid
  34. The Battery
  35. The Vacuum Pump
  36. Magnets
  37. The Light Bulb
  38. Copper Wire
  39. The Generator
  40. The Vacuum Tube
  41. The Electric Arc Furnace
  42. Pure Silicon
  43. Semiconductors and the Transistor

Do them roughly in this order. See it on the tech tree →

Why it matters

A The Vacuum Tube can switch and amplify, but it is a glass bottle with a glowing filament inside. It needs a good vacuum, burns watts of power just to stay warm, takes seconds to start, and wears out after a few thousand hours. A semiconductor device does the same jobs with a speck of crystal: no vacuum, no heater, almost no power, and it can last for decades.

Semiconductors come in three steps of difficulty, and each is worth having:

  1. Crystal detectors (1906): a lump of natural mineral touched by a fine wire. They let a Radio receiver work with no battery at all. Anyone can make one in an afternoon.
  2. Rectifiers (1920s): plates of oxidised copper that turn alternating current from a The Generator or The Transformer into direct current, for charging a The Rechargeable Battery or running Electrolysis and Electroplating. A week's work with a good furnace.
  3. Transistors (1947): a crystal so pure, and so precisely spoiled with impurities, that a small current in one wire controls a big current in another. These are the foundation of Integrated Circuits, the modern The Computer, Solar Cells and nearly all of electronics. Realistically, they need a team, Pure Silicon or germanium, and a lot of patience.

Be honest with yourself about the third step. Vacuum tubes and relays (The Relay Computer) will do almost everything a transistor can, only bigger and hungrier. Make transistors when you have the purity to make them; until then, the first two steps are cheap and useful.

How it works

Conductors, insulators — and the in-between

In a metal, some electrons are loose and drift freely: a little voltage pushes a big current. In glass or quartz, every electron is held tight in a bond between atoms: almost no current flows. Semiconductors — silicon, germanium, galena, copper oxide, selenium and others — sit in between. Their electrons are mostly held, but heat or light can shake a few loose. That is why a semiconductor, unlike a metal, conducts better when warm or when light falls on it.

Doping

Silicon and germanium atoms each have four outer electrons, and in a crystal each atom shares them with four neighbours, in a perfectly regular lattice. Now replace a few atoms:

  • Put in an atom with five outer electrons — phosphorus, arsenic or antimony — and the fifth has no bond to join. It wanders free and carries current. This is n-type (n for negative).
  • Put in an atom with three — boron, aluminium, gallium or indium — and one bond is short an electron. That gap, called a hole, is filled by a neighbouring electron, which leaves a gap behind it, and so the hole moves through the crystal like a positive charge. This is p-type (p for positive).

Adding impurities on purpose is called doping, and the amounts are astonishingly small. About one dopant atom per million silicon atoms makes the crystal conduct many thousands of times better. This is also why stray impurities ruin everything: the crystal must first be made purer than almost anything else people make, and only then spoiled exactly as you want.

SiSiSiSiSiSiSiSiSi SiSiSiSiPSiSiSiSi SiSiSiSiBSiSiSiSi Pure siliconevery electron held in a bond n-typea phosphorus atom (5 outer electrons) p-typea boron atom (3 outer electrons) so almost no current flows:a poor conductor the 5th electron is spare andwanders free: it carries current one bond is short an electron: a"hole" that moves like a + charge Forward: p side to + current pn thin zone +− Holes and electrons are pushed into the junction and meet: current flows once you pass about 0.6 V (silicon). Reverse: p side to − pn wide empty zone −+ Holes and electrons are pulled away; the zone between has nothing to carry current: almost none flows.
Fig. 1 Inside the crystal. Pure silicon holds every electron in a bond. A phosphorus atom brings a spare electron (n-type); a boron atom leaves a bond one short — a "hole" (p-type). Where p meets n, current can flow one way but not the other.

The p-n junction: a one-way valve

Grow a crystal that is p-type on one side and n-type on the other. Near the boundary, free electrons from the n side fall into holes on the p side, and both disappear, leaving a thin empty zone — about a thousandth of a millimetre — with nothing in it to carry current.

  • Connect the p side to + and the n side to −. Holes and electrons are pushed towards the junction, the empty zone shrinks, and once the voltage passes about 0.6 V for silicon (about 0.3 V for germanium) current flows freely. This is called forward.
  • Turn the battery round. Holes and electrons are pulled away, the empty zone widens, and almost nothing flows — until, at some much higher voltage (tens to hundreds of volts), the junction breaks down.

A one-way valve for current is a diode, or rectifier. A fine metal point pressed onto a semiconductor crystal makes a similar one-way barrier, which is why the cat's-whisker detector works. So does the boundary between copper and a skin of copper oxide grown on it.

The transistor

Make a sandwich — n-p-n or p-n-p — with the middle layer extremely thin: a hundredth of a millimetre or less. Call the three layers emitter, base and collector. With no current into the base, the base-collector junction is reverse-biased and blocks. Push a small current into the base, and the emitter floods the thin base with carriers; nearly all of them shoot straight through into the collector. Result: a small base current controls a collector current 20 to 200 times larger.

That one property gives you the two things all of electronics is built on:

  • A switch: base current on, lamp on; off, off — exactly like a relay, but in a millionth of a second instead of a hundredth, with no moving parts. Gates, adders and memory built this way are the The Computer.
  • An amplifier: a faint wavering signal on the base becomes a strong copy at the collector, as with the triode The Vacuum Tube (see Amplifiers and Oscillators).
An alloy-junction transistor (p-n-p) cut through the middle; thickness greatly exaggerated ECB p-type layersregrown from the melt Emittersmall indium bead Basen-type germaniumwafer, 0.1 mm Collectorlarger indium bead base layer left between the two p-type layers: about 0.01–0.02 mm Base contact: a ring of tin or solder on the wafer Used as a switch symbol for an n-p-n transistor 6 V CEB switch 10 kΩ 50–100 × bigger small base current,about 0.5 mA Close the switch: a tiny current into the base lets a big current flow from collector to emitter, and the lamp lights. A p-n-p transistor works the same way with the battery turned round.
Fig. 2 Left: an alloy-junction transistor, the most approachable kind to make — two beads of indium melted into opposite faces of a thin wafer of n-type germanium. Right: a transistor used as a switch.

What you need

Route Materials Tools
Crystal detector Galena, or pyrite, chalcopyrite, zincite, or a lump of silicon or carborundum; 0.1–0.2 mm springy wire (brass, bronze, steel, or gold); brass; solder Pliers, a wooden base, a cell and a galvanometer (Measuring Electricity) to test
Copper-oxide rectifier Copper sheet 1 mm thick; lead sheet; dilute acid; an insulating rod A The Kiln or muffle furnace reaching 1,000–1,050 °C; tongs; a bucket of water
Transistor Germanium or silicon purified to about one part in a billion (Pure Silicon); indium, aluminium, antimony or phosphorus as dopants Furnaces with steady temperatures to ±5 °C; hydrogen or nitrogen gas; acids for etching; a The Microscope; fine gold or tinned copper wire; clean room conditions (Clean Rooms)

Where to find it

  • Galena: lead sulfide, the main ore of Lead. Very heavy, bright steel-grey, breaking into perfect little cubes with mirror-bright faces. Found in veins with quartz and calcite, often with zinc ore. The best detector pieces are freshly broken, coarse-crystalled lumps.
  • Pyrite ("fool's gold"): brassy yellow cubes, harder than steel. Chalcopyrite: brassier, softer, often tarnished blue-purple. Both work as detectors, less sensitively than galena but holding their adjustment better.
  • Zincite: red to orange zinc oxide, rare in nature. A zincite crystal touched by a chalcopyrite point (the "perikon" detector) was robust and popular.
  • Silicon: even rough 98% silicon from the arc furnace (Pure Silicon) makes a fine, stable detector. Carborundum (silicon carbide) is made by heating sand and coke to about 2,000 °C in an The Electric Arc Furnace; see Abrasives and Grinding Stones.
  • Germanium (full route in Germanium, Gallium and Compound Semiconductors): never found as a metal and rare in ores. It was first obtained in quantity from the flue dust of zinc smelters and from the ash of certain coals. From such residues, hydrochloric acid (Hydrochloric Acid) distils off germanium chloride (it boils at about 85 °C), which is turned to oxide with water and reduced to metal with hydrogen (Hydrogen, Oxygen and Gases) at about 650 °C. Germanium melts at 938 °C — far easier than silicon at 1,414 °C — which is why the first transistors were germanium.
  • Dopants: phosphorus from bone ash or rock phosphate (Chemical Fertilisers); antimony from stibnite (soft, grey, needle-like crystals); boron from borax; aluminium from Aluminium. Indium is recovered from zinc-smelting residues and is genuinely hard to get.

Method 1: The cat's-whisker detector

The cat's-whisker detector Insulated handle Arm on a ball jointbrass; lets you move the point Cat's whiskerspringy wire 0.1–0.2 mm,coiled so it presses lightly Crystalgalena or silicon brass cup, crystal held in solder terminals Testing it arrow symbol = the easy direction Forward cell galvanometer swings hard Reversed cell little or no swing
Fig. 3 The cat's-whisker detector. A fine springy wire touches a lump of crystal; you move it around until it finds a sensitive spot. Test it with a cell and a galvanometer: current flows well one way, hardly at all the other.
  1. Break the crystal to expose fresh faces. Old, tarnished surfaces work badly. A piece 5–10 mm across is plenty.
  2. Mount it in a small brass cup. Pour in a little molten solder (tin-lead, see Soldering and Brazing) and press the crystal into it as it cools, leaving the top half exposed. Do not overheat galena: it gives off lead and sulfur fumes and loses sensitivity. A spring clip that grips the crystal also works.
  3. Make the whisker: 3–4 cm of springy wire 0.1–0.2 mm thick, coiled into 3–4 loose turns like a tiny spring, with a sharp point. Fix the other end to a brass arm that can swing and tilt on a ball joint, with an insulating handle so your hand doesn't add noise.
  4. Test it: connect a single cell (zinc–copper, about 1 V), a thin-wire galvanometer, and the detector in a loop. Move the whisker gently over the crystal. At most points the galvanometer reads the same both ways. At a sensitive spot it reads much more with the cell one way round than the other — ten times or more. Mark the way round that gives the big reading: the crystal is now a diode.
  5. Use it in a crystal set (Radio). Its real test is listening: with antenna, tuning coil and earphone, search for the spot that gives the loudest signal. A good spot can last days; a knock loses it.

Tip In the Second World War, prisoners and soldiers with no crystals made "foxhole radios" using a blued (heat-darkened) razor blade as the crystal and the graphite lead of a pencil, held by a safety pin, as the whisker. The oxide skin on the steel acts as the semiconductor. Rusty iron, burnt copper and some coloured mineral grains will all do it weakly.

Method 2: The copper-oxide rectifier

A thin layer of red copper oxide grown on copper conducts well in one direction only. Discs of it were used in their millions from the 1920s to charge batteries and run meters. They are clumsy for radio but excellent for power.

  1. Cut discs of pure copper sheet 1 mm thick, 3–5 cm across, with a hole in the middle for a mounting rod. Clean them bright with fine sand and then dilute acid; do not touch the faces with your fingers.
  2. Heat the discs in a furnace in air at about 1,000–1,030 °C — bright orange-yellow, just short of copper's melting point of 1,085 °C — for about 5–10 minutes. A thick black-and-red scale forms. Watch closely; at the edges the copper must not start to melt.
  3. Cool and quench: take them out, let them cool in air for a minute or two to a dull red (about 500–600 °C), then plunge them into cold water. Much of the outer black scale (cupric oxide) cracks off.
  4. Strip the black layer: dip in dilute acid (see Acids, Bases and Testing) for a few seconds at a time and rinse, until one face shows an even, glassy brick-red layer of cuprous oxide over the copper. Scrape the oxide off the other face and the edges, so only one face carries it. This step needs practice; the recipe varied between factories and is the part most likely to need your own trials.
  5. Make the contact: press a disc of soft lead foil (or a graphite paste painted on and dried) hard against the red face. Clamp a stack together on an insulated rod: copper disc, oxide, lead, copper disc, oxide, lead, and so on, with brass end plates for terminals.
  6. Test: current flows easily when the oxide side is positive and the copper negative, and very little the other way.

Each disc blocks only a few volts — roughly 5 V at best, often less — before it leaks badly, so stack one disc for every 3–5 V of the highest voltage it must block, and test the stack before trusting it. A 4-cm disc passes a few hundred milliamps without overheating; use more discs in parallel, or bigger ones, for more. Fins of thin copper between discs help them shed heat.

Method 3: Transistors

This is an outline of the most approachable route, not a recipe you will get right the first time. Every step was a hard-won discovery, and every factory had its own secrets.

First, a single crystal

Transistors must be made in a single crystal — one unbroken lattice — and of extreme purity. Zone refine the germanium or silicon: lay a bar in a clean graphite or quartz boat under hydrogen or nitrogen, and move a narrow molten zone slowly from one end to the other, a few centimetres an hour, with a ring heater. Impurities prefer the liquid and are swept to the far end. Ten to twenty passes, cutting off the dirty end each time, bring germanium to better than one foreign atom in a billion. Then pull a single crystal from the melt on a seed, adding a measured pinch of dopant (antimony for n-type germanium). See Pure Silicon for crystal growing.

Test of purity without instruments: very pure germanium and silicon conduct poorly at room temperature but much better when warmed by your hand or a flame. A crystal that conducts well even when cold is still full of impurities.

The point-contact transistor

The first transistor (Bell Laboratories, December 1947) was two gold contacts, about 0.05 mm apart, pressed by a spring onto a block of n-type germanium. A strip of gold foil was wrapped round a plastic wedge and slit at the tip with a razor to make the two points. Short pulses of current through the collector point "formed" it. Such devices are fragile and vary wildly, but they work with germanium of ordinary chemical purity, and they were the first proof that it could be done.

The alloy-junction transistor

  1. Slice n-type germanium into wafers about 0.1 mm thick (grind and lap a thicker slice with fine abrasive on glass, Abrasives and Grinding Stones). Etch the surface clean in a mixture of acids.
  2. Place two dots of indium on opposite faces, exactly opposite each other: a small one (about 0.4 mm) for the emitter, a bigger one (about 0.6 mm) for the collector. Use a jig to hold them.
  3. Heat in hydrogen or nitrogen to about 500–550 °C for a few minutes. The indium melts and dissolves germanium beneath it. On cooling, germanium regrows out of the melt carrying indium with it: a p-type layer under each dot. Between the two p layers is left a thin n-type base, ideally 0.01–0.02 mm.
  4. Attach leads: fine wires soldered into each indium bead, and a ring of tin solder on the wafer for the base. Etch again to clean the edges of the junctions, dry, and seal in a small glass or metal case with a drying agent.
  5. In silicon, the same trick works with aluminium instead of indium, at about 600–700 °C.

Test: use a cell and galvanometer. Base to emitter and base to collector should each behave as a diode. Then set it up as a switch (figure above), with a 3–6 V battery and a small lamp. Touch the base through a resistor of 5–10 kΩ (a long piece of thin iron wire, or a pencil line on paper): the lamp should light. If it lights equally with the base open, the junctions are leaky.

How to tell it worked

  • Diode test: with one cell and a galvanometer, a good diode shows at least ten times more current one way than the other. A good silicon junction shows almost nothing in reverse.
  • Detector test: a crystal set with your detector picks up a station loudly enough to hear in a quiet room.
  • Rectifier test: put the rectifier stack between a hand-cranked AC generator and a galvanometer. Without it the needle shivers around zero; with it the needle stands steadily to one side.
  • Transistor test: the lamp lights only when the base is fed; the lamp current is many times the base current (compare galvanometer readings).

Note Troubleshooting. Detector gives the same reading both ways → no sensitive spot yet: keep searching, break a fresh face, try another crystal, or lighten the whisker's pressure. Copper-oxide disc conducts both ways → the oxide is cracked or too thin, the black layer is left on, or oxide on the back face is shorting round the edge. Make another; grow the oxide longer. Copper-oxide disc hardly conducts either way → black cupric oxide left on, or bad contact: press the lead harder. Transistor junctions both leak → surface dirt or moisture. Etch, rinse in the purest water you have, dry and seal. No transistor action, but two good diodes → the base is too thick. The two p-layers must almost meet. Everything changes as it warms up → normal for germanium; keep it cool and keep currents small.

Dangers

Danger Etching acids. Semiconductor work uses strong acids. Hydrofluoric acid in particular (made from fluorite and Sulfuric Acid) passes through skin without pain at first and then destroys tissue and bone and can stop the heart. Never use it without heavy rubber gloves, a face shield and plenty of running water, and have calcium gluconate gel within reach before the bottle is opened. After any splash, wash under running water for about 5 minutes, then rub in the gel at once and keep rubbing, and get medical help (Fluorspar and Fluorine Compounds). Chalk paste is useless. Prefer other etches when you can.

Danger Hydrogen used to protect hot crystals forms an explosive mixture with air. Purge the furnace tube with nitrogen or carbon dioxide before heating and after; burn the hydrogen off at the exit in a small flame; never let air back into a hot tube full of it.

  • Lead and arsenic. Galena dust is poisonous; wash hands, do not grind it indoors. Never use arsenic as a dopant — phosphorus and antimony do the same job. Germanium and indium compounds should not be breathed.
  • Hot copper and scale spit when quenched. Wear eye protection and stand back.
  • Furnace burns: see The Kiln.

Going further

  • Light from crystals. In 1907 H. J. Round noticed that a carborundum crystal glowed yellow when current passed through it — the first light-emitting diode (see Light-Emitting Diodes). The same junctions, run backwards, turn light into current: see Solar Cells. Selenium and copper oxide made the first light meters for Photography.
  • Better diodes stop relay "sneak paths" and quench coil sparks in a The Relay Computer.
  • Many transistors on one crystal: Integrated Circuits.
  • Computers: a transistor flip-flop holds one bit; a few thousand transistors make a working processor (The Computer).

How it was first done

In 1874 the German physicist Ferdinand Braun found that some metal-sulfide crystals conducted better one way than the other. Around 1900 the Indian scientist Jagadish Chandra Bose used galena point contacts to detect radio waves. In 1906 the American Greenleaf Whittier Pickard patented the silicon detector and Henry Dunwoody the carborundum detector; for two decades the crystal set was the radio of ordinary people. Copper-oxide rectifiers were introduced by Lars Grondahl and Paul Geiger at Westinghouse in the mid-1920s.

Radar during the Second World War needed better detectors, and the work on purified silicon and germanium, especially at Purdue University and Bell Laboratories, laid the ground for what came next. On 16 December 1947, at Bell Labs, John Bardeen and Walter Brattain made the point-contact transistor amplify; they demonstrated it to their managers a week later. William Shockley, their group leader, worked out the theory of the junction transistor in early 1948, and grown-junction transistors were made in 1950–51. Gordon Teal and John Little grew single crystals; William Pfann invented zone refining around 1951; alloy-junction transistors were made by General Electric and RCA in 1951–52, and Teal, at Texas Instruments, made the first commercial silicon transistors in 1954. Bardeen, Brattain and Shockley shared the Nobel Prize in Physics in 1956. Within twenty years, transistors had replaced vacuum tubes almost everywhere.