Heavy honey-coloured grains of monazite in beach and river sand hold a family of seventeen look-alike metals. Crack the sand with lye or acid, split off cerium and yttrium, and you can make lighter flints and fire steels that spark when wet, the white-hot oxides of gas mantles, a polish that brings lenses to a shine fast, and powders that glow in the dark or turn ultraviolet and electron beams into light.

Difficulty
●●●●●
Time
Days to concentrate the sand and crack it; weeks of patient chemistry for the separations; a day to cast flints once you have mischmetal
Steps from zero
15 prerequisites →

You need first

Identifying SubstancesNitric Acid

This unlocks

EDTA, Extractants and Chelating AgentsSeparating the Rare EarthsPermanent Magnets
The full path from nothing — 15 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. The Kiln
  6. Lime
  7. Lye and Potash
  8. Fermentation
  9. Glass
  10. Acids, Bases and Testing
  11. Saltpeter
  12. Laboratory Glassware
  13. Sulfuric Acid
  14. Identifying Substances
  15. Nitric Acid
  16. Rare Earths, Cerium and Phosphors

Do them roughly in this order. See it on the tech tree →

Why it matters

The rare earths are seventeen metals: lanthanum, cerium, neodymium and their relatives, plus yttrium and scandium. They are not actually rare. Cerium is about as common in the Earth's crust as copper. But they are scattered thinly, and they are so alike chemically that it took chemists a century to tell them apart. A rebuilding society can get a surprising amount from them without separating all seventeen:

Be realistic. Mixed rare earths, cerium, a yttrium-rich fraction and mischmetal are within reach of this book's chemistry. Every element pure is a much bigger job; that took 20th-century ion exchange and solvent extraction, described in Separating the Rare Earths. And the simplest phosphor needs no rare earths at all, only seashells and sulfur.

How it works

Why they are alike. All rare earths form ions with the same charge, three positive, and nearly the same size. They are like seventeen siblings in identical clothes. The few handles to grab them by are:

Handle Which ones How you use it
Insoluble oxalates All rare earths Oxalic acid throws them all down even from acid solution, leaving iron, aluminium and most other metals behind
Cerium can be oxidised to a four-positive form Cerium only Ceric compounds dissolve far less easily than the others, so cerium can be filtered off
Double sulfates with sodium "Light" group: lanthanum, cerium, praseodymium, neodymium, samarium They crystallise out of a salt-rich solution; the "heavy" group and yttrium stay dissolved
Europium can be reduced to a two-positive form Europium only It then behaves like barium and precipitates as an insoluble sulfate
Small differences in solubility Each pair of neighbours Fractional crystallisation, repeated hundreds of times (historic, slow)

Thorium, a radioactive metal, travels with them in monazite and must be removed and kept safe (Detecting Radiation).

Sparks. Cerium and lanthanum are soft metals that burn in air at only about 150–180 °C. A steel edge scraping mischmetal tears off tiny shavings that heat up from friction and burst into flame in mid-air, much hotter than steel sparks. Pure mischmetal is too soft and smears instead of chipping. About 20–30 % iron makes it hard and brittle enough to crumble into sparks. This alloy is ferrocerium.

Glow. A phosphor is a crystal with a few foreign atoms, called activators, perhaps one in a thousand. Light or electrons lift the activator's electrons up; as they fall back, they give off light of their own colour. In some crystals the electrons get stuck in "traps" and leak out slowly, so the powder glows for minutes or hours afterwards: phosphorescence. Traces of iron, nickel or cobalt kill the glow, so purity matters most.

What you need

Item Use Notes
Monazite concentrate, a few kilograms Raw material See below
Caustic soda (Lye and Potash) Cracking Or concentrated Sulfuric Acid
Hydrochloric Acid, Nitric Acid Dissolving
Oxalic acid (Oxalic Acid) Precipitating Made by heating sugar with nitric acid, or from wood sorrel salt (below)
Sodium sulfate (Glauber's salt) Double sulfates By-product of Hydrochloric Acid making
Bleach (Chlorine and Bleach) Oxidising cerium
Ammonium chloride (sal ammoniac) Drying the chlorides Ammonia
Iron or graphite crucible, carbon rod, low-voltage DC supply of 100–500 A Mischmetal Electrolysis, The Generator
Clay or porcelain crucibles and dishes, glass beakers, filter cloth Throughout Laboratory Glassware
A radiation detector, even a simple electroscope Checking residues Detecting Radiation

Oxalic acid. Warm 1 part of sugar with 5 parts of Nitric Acid, of the strength used for metal work, in a large porcelain dish outdoors. It foams and gives off choking brown fumes. When the fumes stop, cool it: colourless needle crystals of oxalic acid form. Recrystallise from water. Or boil wood sorrel leaves, strain, add lime water, and collect the white calcium oxalate. Treat that with dilute sulfuric acid to free the oxalic acid. Oxalic acid is poisonous; label it.

Where to find it

  • Monazite. Heavy, small, honey-yellow to reddish-brown grains with a resinous shine, in beach and river sands below granite country, with black magnetite and ilmenite, white zircon, garnet and tin ore. Most gold pans and tin streams show some (Gold and Silver, Titanium). It is about 5 times as heavy as water; quartz is 2.7.
  • Xenotime. Similar yellow-brown grains, rich in yttrium and the heavy rare earths. It occurs in granite pegmatites and in the same sands.
  • Bastnaesite. A waxy yellow to reddish-brown mineral in carbonatites, odd carbonate-rich igneous rocks that look like coarse marble, often with fluorite and barite. It fizzes slowly in warm acid.
  • Ion-adsorption clays. In some warm, wet regions, weathered granite clays hold rare earths so loosely that a strong salt or ammonium sulfate solution washes them out.

Concentrating monazite sand. Pan or sluice to get the heavy fraction (Mining and Tunnelling). Pull out magnetite with a lodestone or strong magnet. A very strong The Electromagnet then lifts ilmenite first and, held closer, monazite, leaving zircon and quartz. Check under a lens on a white plate for the yellow-brown resinous grains; a rich batch makes a radiation detector click clearly faster.

Method 1: Cracking and separating (outline)

Monazite sandground fine, wet strong hot lye, 140–150 °C, 3–4 h Hydroxide sludgerare earths + thorium Liquid: sodium phosphatewash off; lime makes fertiliser + lye dilute hydrochloric acid, just slightly acid Rare-earth solutionchlorides Undissolved: THORIUMradioactive: keep wet, seal, bury alkali + bleach (cerium turns yellow),then weak nitric acid Solutionall except cerium Undissolved: CERIUMyellow; polish, mantles, flints saturate with sodium sulfate, overnight Solution: yttrium groupyttrium, heavy rare earths Crystals: light grouplanthanum, neodymium, praseodymium Each fraction: dissolve in acid, add oxalic acid, calcine the oxalateat 800–900 °C to oxide; iron and other metals stay behind in the liquid Mixed oxides with the thorium removed (before splitting) make mischmetal
Fig. 1 Separating the rare earths in outline. Monazite is cracked with hot caustic soda; the phosphate washes away as a useful salt. Acid dissolves the rare earths but leaves radioactive thorium behind. Oxidising lets cerium be filtered off. Sodium sulfate splits the rest into a light group and a yttrium group, and oxalic acid brings each down for calcining to oxide.

Cracking

  1. Grind the monazite concentrate as fine as flour, wet, so there is no radioactive dust.
  2. Digest 1 kg of monazite with 1.5 kg of caustic soda dissolved in about 1 litre of water, to make a thick, very strong lye. Do it in an iron pot at 140–150 °C, just above the boiling point of the strong lye, stirring, for 3–4 hours. The grains turn into a fine, pale paste.
  3. Dilute with hot water and settle. The liquid holds trisodium phosphate, a strong cleaning salt. Stirred with lime, it gives calcium phosphate for fertiliser and turns back into lye you can use again. The solid is mixed rare-earth and thorium hydroxides. Wash it several times.

The acid route is the alternative. Heat ground monazite with about twice its weight of concentrated sulfuric acid at 200–250 °C for several hours, cool it, and stir it into ice-cold water. Rare-earth sulfates dissolve better cold than hot. This route is cheaper in alkali but harsher, with acid fumes.

Removing thorium

Stir the wet hydroxides into water and add dilute Hydrochloric Acid slowly, testing with litmus, until the solution is just slightly acid and no more dissolves. That is about pH 3–4; see Acids, Bases and Testing. The rare earths dissolve. Thorium, along with some iron and much of the cerium if it has oxidised, stays as an undissolved sludge. Filter.

Warning The thorium sludge is radioactive, and so are the liquors that carry radium from it. Keep it wet, store it in sealed clay pots, and bury it in a marked, clay-lined pit far from wells, homes and fields (Detecting Radiation, Sanitation and Germs). Never use it in glazes, mantles or fertiliser.

Splitting off cerium

  1. Make the rare-earth chloride solution alkaline with lye or soda ash so all the hydroxides fall out again.
  2. Stir in bleach solution, or bubble chlorine through it (Chlorine and Bleach), or simply dry the hydroxides in air at 100–120 °C for a day. The cerium oxidises: the white hydroxide turns creamy yellow.
  3. Stir the mass into water and add dilute nitric acid slowly to about pH 3–4. Lanthanum, neodymium, praseodymium and the rest dissolve. Ceric hydroxide, the yellow part, stays. Filter.
  4. Repeat steps 2–3 on the ceric solid once more for purer cerium.

Light and yttrium groups

Into the solution of the other rare earths, stir solid sodium sulfate until no more dissolves, and leave it overnight. A white crystalline powder of double sulfates of the light group falls out: lanthanum, praseodymium, neodymium, samarium. Yttrium and the heavy group stay in solution. Boil the double sulfate with lye to turn it back to hydroxide.

Oxalate and oxide

For each fraction: dissolve it in dilute hydrochloric or nitric acid, and add oxalic acid solution until no more precipitate forms. A heavy white or pinkish oxalate settles; iron and other impurities stay dissolved. Wash it, dry it, and calcine it in a clay dish at 800–900 °C (cherry-red to orange) for 2 hours:

Fraction Oxide colour
Cerium Pale cream-yellow (white when very pure)
Light group with praseodymium Brownish to black, due to praseodymium
Neodymium-rich ("didymium") Bluish-grey; its salts are lilac
Yttrium group White to faint pink

Separating neighbours further means fractional crystallisation: crystallise a salt, split the first crystals from the rest, and repeat on each part hundreds of times. It needs only dishes and patience. Charles James took about 15,000 recrystallisations to purify thulium.

Europium (for red phosphors). Dissolve the light-and-middle fraction in dilute hydrochloric acid, and run it through a tube packed with zinc granules coated with a little mercury (Mercury). This turns europium alone into its two-positive form, which behaves like barium. Add a little sulfuric acid at once: europium sulfate comes down with any barium. Air turns it back within minutes, so work quickly under a blanket of carbon dioxide. This is the method of H. N. McCoy (1936).

Method 2: Mischmetal and ferrocerium

Mischmetal

Mischmetal (German for "mixed metal") is the rare earths of monazite or bastnaesite as metal, without separating them: about 50 % cerium, 25 % lanthanum, 15–18 % neodymium and 5 % praseodymium. You make it by electrolysing the molten chlorides.

  1. Make dry chloride. Dissolve mixed oxides or hydroxides from which the thorium has been removed in hydrochloric acid and boil it to a thick syrup. Plain drying turns it into useless oxychloride. Instead, stir in 2–3 parts of ammonium chloride for every part of rare-earth chloride, dry it slowly, and heat it gradually to about 400 °C in a covered iron or clay dish until white ammonium chloride fumes stop. What is left is dry rare-earth chloride. Keep it sealed; it soaks up water from the air in minutes.
  2. Cell. Use an iron or graphite crucible 15–25 cm across, heated from outside in a furnace (Electric Kilns and Furnaces). Mix the chloride with about a fifth of its weight of salt and potassium chloride, which helps it melt and conduct. A carbon rod anode (Lampblack and Carbon Black) dips into the middle. An iron rod through the bottom, or the crucible itself, is the cathode.
  3. Run it. Melt the bath at 850–900 °C, bright cherry-red to orange. Pass direct current, a few hundred amperes for a crucible this size, at about 8–12 V. Chlorine bubbles off the anode; draw it away with a hood and chimney (Chlorine and Bleach). Liquid mischmetal collects at the bottom.
  4. After an hour or two, pour or ladle the metal into an iron mould under a cover of molten salt, or let it freeze in the crucible and break it out.

Mischmetal is a soft, silvery metal that tarnishes yellow-brown in damp air. Small amounts go into steel and cast iron to clean out sulfur and oxygen and toughen the metal (The Blast Furnace and Cast Iron, Alloy and Stainless Steels).

Ferrocerium flints and rods

Casting Salt coverkeeps air offMischmetal+ 20–30 % iron,about 800 °C split steel mould, preheated and oiled:rods and fine flint channels Fire steel and lighter flint Handlewood or antlerRod 6–12 mm × 8–12 cmblack lacquer: scrape off firstKnife spine or strikersparks Toothed steel wheel6–7 mm, hardenedFlint 2.4–3 mm × 4–6 mmferrocerium, a few thousand lightsSpringpresses flint up to the wheel
Fig. 2 Ferrocerium. Mischmetal and iron are melted together under a cover of salt and cast in a split steel mould. A thick rod in a handle becomes a fire steel, scraped hard with a knife spine; a thin flint, pushed by a spring against a toothed steel wheel, lights a lighter.
  1. Melt 70–80 parts of mischmetal in a clay-graphite or iron crucible under a cover of melted salt (salt with potassium chloride, or calcium chloride) to keep the air off. Melt at about 800 °C, cherry red.
  2. Stir in 20–30 parts of clean iron in small pieces: soft wire, nails or turnings. Iron dissolves into the rare earths well below its own melting point. Optionally add 2–4 parts of magnesium (Magnesium) for more sparks.
  3. Cast at once into preheated, oiled steel moulds:
    • Lighter flints: rods 2.4–3 mm across. Cut them into pieces 4–6 mm long. One flint gives a few thousand lights.
    • Fire steel rods: 6–12 mm thick and 8–12 cm long. Bed one end in a wooden or antler handle with resin.
  4. Let them cool under the salt, then wash off the salt and dry them at once.
  5. Seal each rod with a thin coat of lacquer or wax. Ferrocerium slowly crumbles in damp air. The black coat on bought rods is this protection; scrape it off before first use.

Using a fire steel. Hold the rod against the tinder and scrape firmly down its length with the spine of a knife or a hardened steel striker, pulling the rod back rather than pushing the striker forward, so you do not scatter the tinder. It works wet, cold and at altitude (Fire).

Good and bad flints. A good flint gives a fat, yellow-white shower from a light stroke, and the sparks run 10–20 cm. Too little iron gives a soft flint that smears and clogs the lighter wheel. Too much iron (over about 35 %) gives a hard flint with few, short, red sparks. Grey, crumbly rods with black specks contain oxide; the salt cover was too thin.

Method 3: Cerium oxide polish and mantle oxides

Cerium polishing powder. Calcine the purest cerium oxalate or hydroxide at 900–1,000 °C, orange to yellow heat, for 2 hours. Grind it gently wet and settle it in water to keep the fine grades, as with any abrasive (Abrasives and Grinding Stones). Use it as a thin cream on a pad of felt or pitch, as when polishing lenses (Optical Glass and Achromatic Lenses, The Telescope). Glass comes up bright in a third to a half of the time that rouge needs, and the powder washes off clean. A good powder is pale cream to pinkish-buff, free of grit (rub a pinch between two glass slides and look for scratches), and non-radioactive, so check it.

Mantle oxides. Dissolve 99 parts of yttria and 1 part of ceria (oxides of the yttrium group and cerium, by weight) in dilute nitric acid, and use the solution to soak cotton mantle socks (Lanterns, Gas Lamps and Lighters gives the rest). Lanthanum-rich oxide can stand in for yttria but gives a weaker, shorter-lived mantle. Never use the thorium sludge, however well the old mantles glowed.

Method 4: Phosphors

A phosphor is a glowing powder. Three kinds, from easiest to hardest:

Shells + sulfureasiest covered, red heat, 1 h Zinc sulfide+ trace of copper fired 900–1,000 °C,tightly covered Strontium aluminate+ europium, dysprosium buried in charcoal,1,300–1,400 °C Luminous painton a dial Phosphor in varnish1 : 1–2, 0.2–0.3 mmwhite undercoaton metal or card Glow after the light goes out 010 min1 hourseveral hours shells + sulfurzinc sulfidestrontium aluminate
Fig. 3 Three phosphors. Calcined seashells and sulfur, fired in a covered crucible, give a calcium sulfide that glows for many minutes after daylight. Zinc sulfide with a trace of copper glows bright green and fades fast. Strontium aluminate with europium and dysprosium, fired hot under charcoal, glows for hours. Mixed with clear varnish over a white undercoat, any of them makes luminous paint.

Canton's phosphor: seashells and sulfur

  1. Burn seashells, such as oyster, cockle or mussel, in a hot fire for an hour (Lime). Pick out the purest white pieces and grind them.
  2. Mix 3 parts of this shell lime with 1 part of powdered sulfur (Sulfur).
  3. Pack it into a clay crucible, press on a lid sealed with clay, and fire it at red heat, about 800–1,000 °C, for one hour. Do this outdoors; it gives off choking sulfur fumes.
  4. Cool, break it open, and scrape off the white and whitish parts. Expose them to bright daylight for a minute, then take them into a dark room. They glow a soft yellow-green or blue-white for several minutes, fading over half an hour.

A trace of activator makes it stronger. Add a few drops of bismuth salt solution (about 1 part per 5,000) (Antimony and Bismuth) to the shell lime before firing, for a violet-blue glow. Add manganese for orange. This is the old Balmain's luminous paint. It breaks down in damp air, smelling of rotten eggs, so seal it in varnish.

Zinc sulfide

Zinc sulfide with a trace of copper glows a bright green and fades within a few minutes. With silver it glows blue under electron beams, X-rays and alpha particles. It is made as described in Cathode Rays and Television, from zinc (Zinc and Brass). It is the classic coating for X-ray screens (X-Rays) and for alpha particle counters (Detecting Radiation).

Strontium aluminate (the bright modern glow)

This is the powder in modern exit signs and watch hands. It is about ten times brighter than zinc sulfide and glows for hours. It needs both alumina and two separated rare earths, so it is the last to try.

  1. Mix dry and grind well: 148 g of strontium carbonate (from celestine, as in The Vacuum Tube), 102 g of pure alumina (Alum and Alumina), 3.5 g of europium oxide, 3.7 g of dysprosium oxide (from the heavy fraction), and 5 g of boric acid as a flux (Borax and Boric Acid).
  2. Fire it in a covered alumina or porcelain crucible, buried in charcoal powder inside a larger crucible so the gas around it is reducing, at 1,300–1,400 °C for 2–4 hours (The Kiln, Electric Kilns and Furnaces).
  3. Crush it gently. Hard grinding kills the glow. Sieve it.

It glows yellow-green. It is spoiled by water over time, so keep it in varnish.

Lamp and screen phosphors. Yttrium oxide with about 5 % europium gives the pure red of colour television and three-colour lamps, and terbium gives green. They need very pure separated oxides, so treat them as a later goal (Arc Lamps, Neon and Fluorescent Lights, Flat Screens: LCD and LED Displays).

Luminous paint

Luminous paint is any glow phosphor mixed into a clear binder.

  1. Mix 1 part of phosphor with 1–2 parts of clear varnish (a pale oil, resin or nitrocellulose lacquer; see Pigments, Paints and Varnish, Early Plastics). Stir it; do not grind it.
  2. Paint the dial, switch or sign white first, because the white reflects the glow outward.
  3. Lay the luminous coat 0.2–0.3 mm thick, about two or three brushed coats. Thin coats glow faintly.

Good and bad: a good coat looks even and pale by day and glows evenly in the dark. Grey patches mean iron got into the powder, from an iron mortar, a rusty spoon, or impure shells.

Warning Never use radium or other radioactive paint. Dial painters who licked their brushes in the 1920s died of bone cancer (Detecting Radiation). Charged phosphors glow brightly enough for dials and exit signs.

How to tell it worked

  • Oxalate test for rare earths: a pinch of your product dissolved in dilute acid gives a heavy white precipitate with oxalic acid, and does not redissolve in excess.
  • Cerium: a drop of hydrogen peroxide added to a cerium solution made alkaline with ammonia gives a red-brown to orange colour. Pure lanthanum and yttrium give white.
  • Thorium out: a radiation detector shows no more than background near your oxide.
  • Ferrocerium: a light scrape throws a fat shower of sparks.
  • Phosphor: after a minute of sunlight, it glows clearly in a dark room after your eyes have adjusted for two minutes.

Note Troubleshooting. Monazite will not crack → ground too coarsely, or the lye was not strong or hot enough. Regrind wet and keep it at 140–150 °C. Oxalate precipitate is yellow or brown → iron came through. Redissolve, adjust to slightly acid, and precipitate again. Cerium will not separate → not oxidised. Use more bleach, or dry it longer in air. Mischmetal comes out as black powder, not a pool → wet chloride (oxychloride) or a bath that is too cold. Dry it better with more ammonium chloride; run hotter. Phosphor does not glow → iron, nickel or copper contamination, wrong firing heat, or not enough activator. Use porcelain tools and crucibles only.

Dangers

Danger Thorium and radium. Monazite concentrates, cracking residues and the thorium sludge are radioactive. Breathed or swallowed dust stays in bone and lungs for life. Keep everything wet, work outdoors, wash hands and clothes, store residues sealed and buried away from water, and check with a detector (Detecting Radiation).

Danger Rare-earth metal fires. Mischmetal and ferrocerium filings, grindings and dust catch fire by themselves and burn white-hot. Water makes them worse, because they split it into hydrogen. Smother them with dry sand or dry salt. Grind or cut flints only wet and in small amounts. Keep metal scrap in closed tins under oil.

  • Chlorine from the mischmetal cell and sulfur fumes from phosphor firing choke (Chlorine and Bleach). Use a hood or work outdoors, upwind.
  • Hot strong lye blinds; wear eye protection (Lye and Potash). Molten salt spits if anything wet goes in.
  • Oxalic acid is a kidney poison: 5–15 g can kill. Keep it away from food.

What this unlocks

Flints and fire steels; thorium-free gas mantles; fast lens polishing for Optical Glass and Achromatic Lenses, The Microscope and The Telescope; didymium goggles for Glass workers; luminous dials (Watches and Small Clocks); X-ray screens; fluorescent lamps; and in time rare-earth magnets, pure separated elements (Separating the Rare Earths), Lasers and colour displays (Flat Screens: LCD and LED Displays).

How it was first done

In 1787 the Swedish army lieutenant Carl Axel Arrhenius picked up a heavy black stone at the Ytterby quarry near Stockholm. From it Johan Gadolin separated "yttria" in 1794. In 1803 Berzelius and Hisinger, and separately Klaproth, found "ceria" in a mineral from Bastnäs. Carl Gustaf Mosander split lanthanum and "didymium" from ceria between 1839 and 1841, and Carl Auer von Welsbach split didymium into praseodymium and neodymium in 1885. Auer then invented the gas mantle in the 1880s and 1890s, and patented ferrocerium, "Auer metal", in 1903. His company at Treibach in Austria still makes flints. John Canton described his shell-and-sulfur phosphor in 1768. Frank Spedding's ion-exchange columns at Ames, Iowa, in the 1940s finally made pure rare earths cheap. Yttrium-europium red phosphors arrived with colour television in the 1960s, and a team led by Tadashi Matsuzawa at Nemoto & Co. in Japan patented europium-dysprosium strontium aluminate in 1993.

Source: content/entries/chemistry/rare-earths.md