◆ Rebuild

Part 5 · Cloth and Clothing

Spinning and Weaving Cloth

Twist fibre into yarn with a stick and a weight (the drop spindle), ply it, and weave it on a simple backstrap or warp-weighted loom into plain or twill cloth. Then wash and full it into finished fabric. This is how every piece of cloth was made for ten thousand years.

Difficulty
●●●●●
Time
A day to make a spindle and learn the motion; weeks of practice for even yarn; a tunic's worth of cloth takes roughly 100–250 hours of spinning and 20–50 hours of weaving
Steps from zero
1 prerequisite →

You need first

Cordage and Rope

This unlocks

The WindmillTablet and Band WeavingKnitting, Crochet and NettingThe LoomSewing, Needles and ThreadThe Spinning WheelGliders and AeroplanesBoats and Sails
The full path from nothing — 1 step before this one
  1. Cordage and Rope
  2. Spinning and Weaving Cloth

Do them roughly in this order. See it on the tech tree →

Why it matters

Hides and furs keep you alive, but cloth is lighter, cooler, washable, endlessly reusable and can be made from plants and sheep without killing anything. With cloth you make clothes and bedding (Making Clothes), bandages (Wound Care and Antiseptics), bags and sacks, sieves and filters (Grain, Flour and Bread, Penicillin), sails (Boats and Sails), and the parts of later machines: drive belts (Belts, Chains and Power Transmission), wire insulation (Copper Wire), battery separators (The Battery) and balloon envelopes (Balloons).

Cloth-making has two halves. Spinning turns loose fibre into long, even, strong yarn. Weaving interlaces that yarn into a sheet. Both need only sticks, stones, clay and patience — but they take far more hours than most people imagine. Before machines, spinning was the single biggest consumer of human labour after farming. The The Spinning Wheel and the The Loom chapters describe the faster tools that come next.

How it works

Spinning is the same trick as Cordage and Rope, on a finer scale. You pull out (draft) a thin, even stream of fibres from a mass of prepared fibre, and let twist run into it. The twist makes the fibres grip each other. More twist makes a harder, stronger, thinner yarn; less twist makes a softer, fluffier, weaker one. Short fibres (cotton) need much more twist than long ones (flax, long wool).

A single spun yarn is called a single. Twisted one way, it is energised and wants to kink up. Plying two singles together in the opposite direction balances the twist, exactly as in two-ply cord. As in cordage, twist direction is named Z or S by which way the slant runs. The usual rule: spin singles Z (spindle turning clockwise, seen from above), ply S (anticlockwise).

Weaving needs two sets of threads at right angles:

  • The warp runs the length of the cloth. It is stretched tight on the loom before you start, so it must be strong and smooth — use your best, most twisted yarn, or plied yarn.
  • The weft runs across, passed over and under the warp threads one row (pick) at a time. It can be softer.

Passing the weft over-and-under each thread by hand is slow. Every loom does the same clever thing: it lifts every other warp thread at once, leaving a gap — the shed — through which the weft is passed in one throw. Then it lifts the other half for the return pass. One set of threads is lifted by a shed rod (a stick woven through the warp); the other by heddles (string loops that hold each of the remaining threads to a heddle rod). Lift the heddle rod and its threads come up through the others: that is the second shed.

What you need

Item Size Notes
Spindle shaft 25–35 cm long, 8–10 mm thick, tapered at both ends Straight hardwood, carved and smoothed (Basic Woodworking)
Whorl 4–6 cm across, 20–50 g Fired clay (Pottery), stone, bone or a disc of wood; hole in the exact centre
Distaff A stick 60–100 cm long Holds flax or long wool while spinning
Niddy-noddy A stick 40–50 cm long with two cross-pieces at right angles Winds yarn into skeins
Loom sticks 6–10 straight smooth sticks, 2–3 cm thick, a little longer than the cloth is wide For the backstrap loom
Sword (beater) A flat hardwood blade 3–5 cm wide and 1 cm thick, as long as the loom sticks Opens the shed and beats the weft
Loom weights 30–60 lumps of fired clay or stone, 300–1,000 g each, with a hole For the warp-weighted loom
Fibre Prepared Wool, flax line or tow, or Cotton

Step by step: spinning on a drop spindle

Fibre supplyloosely in back hand Drafting trianglepull fibres out thin Front handpinches, then letstwist run up Half hitch Spun yarnwound on the shaft Whorl20–50 g, 4–6 cm twistruns up spin clockwise (seen from above) for Z yarn draft back TWIST DIRECTION Z twistspin singles S twistply two Z singles The slant of the fibres matches the middlestroke of the letter. Ply the opposite wayto the singles so the twists balance.
Fig. 1 The drop spindle. The spindle hangs and spins from the yarn; your hands pull out a thin triangle of fibre and let the twist run up into it.

Make the spindle

  1. Carve a straight shaft as above, thickest about a third of the way from the bottom, tapering to a point at each end. Cut a small spiral notch or a hook near the top to hold the yarn.
  2. Make a whorl: a disc of clay pinched round a stick to make the hole, dried and fired (Pottery); a flat stone drilled through (Stone Tools); or a slice of wood. It must be balanced — spin it on its shaft like a top and look for wobble.
  3. Push the whorl onto the shaft until it jams tight, about 5–8 cm from the bottom (a low-whorl spindle) — or near the top (a high-whorl spindle; either works).

A heavy spindle (50 g or more) suits thick yarn and long fibre; a light one (15–25 g) suits fine yarn. For cotton, use a light spindle resting on its tip in a small bowl (a support spindle), so the yarn never carries its weight.

Start the yarn

  1. Tie a leader — 50 cm of any finished yarn or cord — to the shaft above the whorl, wind it a few times round the shaft, bring it over the whorl, round the bottom of the shaft once (low-whorl), back up, and catch it in the notch at the top with a half hitch (a single loop slipped over the tip).
  2. Fray the end of the leader and overlap it with a few centimetres of fibre.

Park and draft (learn this way first)

  1. Hold the leader where it joins the fibre. Twist the spindle clockwise (seen from above) with your other hand — a flick of the fingers on the top of the shaft, or a roll down your thigh.
  2. When it has twisted a little, stop the spindle and clamp it between your knees ("park" it).
  3. Pinch the yarn just below the fibre with your front hand. With your back hand, holding the fibre loosely, pull back gently, so a thin, even fan of fibres slides out of the mass: the drafting triangle. Draft about 5–10 cm.
  4. Slide your front hand up, letting the twist run into the drafted fibre. It turns into yarn.
  5. Repeat: draft, release the twist. When the spindle runs out of twist, give it another flick.
  6. When the yarn reaches about arm's length, undo the half hitch, wind the yarn onto the shaft above the whorl in a firm cone, and hitch it again.

Spinning freely

Once the motion is automatic, let the spindle hang and spin while you draft — this is the true drop spindle and is several times faster. Keep the spindle turning the same way all the time; if it stops and turns back, the yarn untwists and drops it. Joining new fibre: lay a fluffy tuft against the fluffy end of the old and let twist run into both.

An experienced spinner makes roughly 50–100 m of medium yarn an hour, more if spinning while walking or tending animals. Good spinners spin all day, at every spare moment.

Ply the yarn

  1. Spin two equal spindles of singles, or wind one long single into a ball and take both ends together.
  2. Hold the two singles together, tie them to the leader, and spin the spindle anticlockwise. The singles wrap around each other.
  3. Balanced yarn: let a 30 cm loop of plied yarn hang. If it hangs straight, the ply is right. If it twists one way, add or remove ply twist.

Single yarns are fine for weft; plied yarn makes the best warp and sewing thread (Sewing, Needles and Thread).

Skein and set the twist

Wind the yarn off the spindle onto a niddy-noddy (in a figure of eight round the four arms), tie the skein loosely in four places, slide it off, and soak it in hot water for 20 minutes. Hang it to dry with a light weight (a stone in a bag) on the bottom. This "sets" the twist so the yarn stops kinking. Wool is washed this way; linen is often boiled (Flax, Hemp and Linen).

Step by step: the backstrap loom

BACKSTRAP LOOM, SIDE VIEW (NATURAL SHED OPEN) Far bartied to a post Shed rodmakes one shed Warp Heddle rodloops lift the other half Swordon edge holds theshed; flat, it beats Wefton a stick shuttle Clothrolled up as it grows Breast bar Backstrapround the hips lean back to tighten
Fig. 2 The backstrap loom. The far end is tied to a post; the near end to a strap round the weaver's hips. Leaning back tightens the warp. The shed rod makes one shed; lifting the heddle rod makes the other.

This is the simplest true loom, still used from Guatemala to Indonesia. It makes cloth up to about 60–80 cm wide and as long as you like.

Wind the warp

  1. Drive two stakes in the ground, the distance apart you want the cloth to be long (say 2 m). Drive a third stake 20 cm in front of one of them.
  2. Tie the warp yarn to the first stake and wind it round the stakes in a figure eight: round the far stake, back to cross between the two near stakes, round the end stake, and back. The X where the threads cross between the two close stakes is the cross: it keeps each thread in order, alternating one over, one under.
  3. Count as you go. For a medium wool cloth 40 cm wide at 8 threads per cm, you need 320 warp threads.
  4. Tie the cross with two lengths of contrasting cord through each half of the X before lifting the warp off the stakes. Slip one loom stick into each end loop.

Set up the loom

  1. Tie one end stick (the far bar) to a post or tree at waist height.
  2. Tie the other end stick (the breast bar) to a backstrap — a strip of leather or a woven band round your hips. Sit on the ground facing the post and lean back to put the warp under tension.
  3. Replace the cord in one half of the cross with the shed rod (a stick 3–4 cm thick, or a cane). Leave it near the far end. The threads on top of it make the natural shed.
  4. Make the heddles. Take a continuous length of strong yarn and a thin stick (the heddle rod). For each warp thread that lies under the shed rod, take a loop of the heddle yarn under that thread and up round the heddle rod. Keep every loop the same length, about 3–4 cm. It takes an hour; do it carefully.
  5. Spread the threads evenly across the breast bar.

Weave

  1. First shed: slide the shed rod towards you. The threads lying over it rise. Turn your sword on its edge in the gap to hold it open.
  2. Pass the weft, wound on a stick (a stick shuttle), right across through the shed. Leave a little slack, laying it at a slant or in a gentle arc (bubbling) so the cloth does not pull narrower.
  3. Beat: turn the sword flat and pull it firmly towards you to pack the weft down.
  4. Second shed: push the shed rod away, and lift the heddle rod. The other half of the threads rise through. Insert the sword, pass the weft back, beat.
  5. Repeat, alternating. Lean back for more tension, forward for less.
  6. As the cloth grows, roll it around the breast bar and re-tie the strap.
  7. Edges (selvedges): keep the weft turning neatly round the outer warp threads, neither tight nor loose. Measure the width every few centimetres.

Method 2: the warp-weighted loom

For wide cloth — blankets, sails, cloaks up to 2–3 m across — Europe and the Near East used the warp-weighted loom for at least 6,000 years.

  1. Build a frame: two posts 2–2.5 m tall, leaning against a wall at about 15°, with a top beam that can turn, resting in forks or holes. Fix a shed bar across the posts about knee height, and brackets above it to hold the heddle bar.
  2. Weave a narrow starting band and sew it to the top beam; its long weft loops become the warp. Hang the warp threads down the front of the loom.
  3. Divide the warp into two layers: the back layer passes behind the shed bar, the front layer in front. Tie small bundles of each layer (10–20 threads, depending on thickness) to a loom weight of fired clay or stone, 300–1,000 g, so each thread carries about 20–40 g. The weights keep the warp tight.
  4. Tie string heddles from the back layer's threads to the heddle bar.
  5. Weave from the top down, beating the weft upwards with a sword. Pull the heddle bar out onto its brackets for one shed; let it rest back for the natural shed.
  6. As the cloth grows, roll it up on the top beam and lower the weights.

Doughnut- and pyramid-shaped clay loom weights, often found in rows where a loom collapsed, are one of the commonest finds in ancient villages.

Weaves

Plain weave (tabby)over one, under one; 2 sheds 2/2 twillover two, under two, step one each row; 4 sheds warp (lengthwise) weft (across) diagonalrib light = warp thread on top dark = weft thread on top Twill packs more threads per cm anddrapes better: warm wool cloth, denim
Fig. 3 Plain weave and 2/2 twill. Plain weave goes over one, under one; twill goes over two, under two, shifting one thread each row, which makes diagonal lines and a thicker, softer cloth.
  • Plain weave (tabby): over one, under one, alternating every row. Two sheds. Strong and firm. For a balanced cloth, use the same number of weft picks per cm as warp threads per cm.
  • 2/2 twill: each weft passes over two warp threads, under two, shifting one thread along on each row. It makes diagonal ribs, packs more threads per cm, drapes better and is warmer. It needs four sheds: on a backstrap or warp-weighted loom, use one shed rod and three heddle rods, each picking up its own set of threads (see The Loom).
  • Basket weave: pairs of threads woven as one in plain weave. Soft, but snags.

Sett (threads per cm) guide: coarse wool blanket 4–6; medium wool cloth 8–12; linen shirting 15–25; fine cotton or silk 30 and up.

Finishing the cloth

Cloth straight off the loom is loose and oily. Finishing makes it fabric.

  1. Secure the ends: knot the warp ends in bundles of 4–6, or hem them.
  2. Wash in warm water with Soap or soapwort (Wool), and rinse.
  3. Full wool cloth (also called waulking): soak it in hot water with soap, or stale urine and fuller's earth (a greasy clay), and pound, knead, trample or rub it for 1–3 hours — on a table, in a trough, or underfoot. The wool fibres felt slightly (Felt), and the cloth shrinks by 10–30 %, becoming thick, dense, windproof and hard-wearing. Check often and stop when it is as dense as you want; you cannot undo it.
  4. Stretch and dry wool cloth on a tenter frame — a frame of poles with rows of hooks ("tenterhooks") — so it dries flat and to an even width.
  5. Raise a nap on wool for warmth and softness by brushing it with dried teasel heads in a frame, then trim the fuzz even with shears.
  6. Linen is not fulled. Wash it, boil it, and bleach it on grass: spread it in the sun, keep it damp, and alternate days of soaking in weak lye (Lye and Potash) with days of soaking in sour milk or whey. It whitens over 4–8 weeks (see Laundry and Bleaching Cloth). Beating damp linen with wooden mallets (beetling) flattens and polishes it.

How to tell it worked

  • Good yarn is even in thickness, without lumps or thin spots, and hard to break with your hands. Unplied singles curl gently on themselves when slack; balanced plied yarn hangs straight.
  • Good cloth has straight, parallel edges, the same width all along, evenly spaced weft, no skipped threads ("floats") and no loose loops at the edges. Hold it up to the light: the spacing should look uniform.

Note Troubleshooting. Yarn drifts apart and the spindle drops → too little twist; let more twist in before drafting further, or draft less fibre at a time. Yarn is wiry and kinks into snarls → too much twist; draft longer between twists. Lumps and thin spots → uneven drafting, or poorly carded fibre (Wool). Cloth gets narrower and narrower → weft pulled too tight; lay it in an arc before beating. Edges loose and loopy → weft too slack at the turns; snug each turn round the edge thread. Threads break in the warp → weak or underspun yarn, or too much tension. Use plied yarn for warp and repair breaks by tying in a new length with a weight. Wrong thread in the shed → a heddle is missing or crossed; stop, find it, and tie a new heddle.

Dangers

  • Repetitive strain. Hours of spinning and weaving bring sore wrists, shoulders, necks and backs. Change position and take breaks; on a backstrap loom, use a wide, padded strap.
  • Fulling with urine is smelly but harmless; work outdoors and wash your hands. Hot water: avoid scalds.
  • Falling loom weights can crush toes; tie them securely.
  • Lye used in bleaching burns skin and eyes (Lye and Potash).

What this unlocks

Yarn and cloth for Sewing, Needles and Thread, Making Clothes, Knitting, Crochet and Netting and bedding. Sacks, sails (Boats and Sails), bandages (Wound Care and Antiseptics), filters and sieves. Faster tools follow: the The Spinning Wheel multiplies spinning speed, the The Loom with treadles multiplies weaving speed, and both lead to Textile Machinery. Woven cloth also feeds Paper (rags), The Battery separators and Copper Wire insulation.

How it was first done

Twisted fibre is at least 40,000 years old (Cordage and Rope), and impressions of woven fabric pressed into clay at Dolní Věstonice in the Czech Republic are about 26,000–27,000 years old. Spindle whorls appear in the Near East with the first farming villages, around 9,000–10,000 years ago, and fragments of woven plant-fibre cloth survive from Çatalhöyük in Turkey from about 9,000 years ago (once thought to be linen, they now appear to be tree bast). A painted bowl from Badari in Egypt, about 6,000 years old, shows a horizontal ground loom. Clay loom weights show that the warp-weighted loom was in use in south-eastern Europe and Anatolia by roughly 5,500 BC, and it remained in use in Scandinavia into the 20th century. The backstrap loom was invented independently in the Americas and East Asia; the Andean weavers of Peru used it to make some of the finest cloth ever made. Until the 1700s, every thread in every garment on earth was spun by hand.

Source: content/entries/textiles/spinning-and-weaving.md