Part 13 · Electricity
Dry Cells and Electric Torches
The Leclanché cell trades the Daniell cell's poisonous blue liquid for sal ammoniac and black manganese ore, and rests between uses without wasting zinc. Packed as a damp paste in a zinc can, it becomes the dry cell that you can carry anywhere. Add a small bulb, a mirror and a switch and you have the electric torch. On a bicycle, a little dynamo against the tyre makes its own light.
- Difficulty
- ●●●●●
- Time
- An afternoon for a Leclanché cell; a week to set up and make a first batch of dry cells; a few days for a torch; two to three weeks for a bicycle dynamo
- Steps from zero
- 15 prerequisites →
This unlocks
—The full path from nothing — 15 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- Hides and Leather
- Fermentation
- Bellows
- Copper Smelting
- Zinc and Brass
- The Battery
- Dry Cells and Electric Torches
Do them roughly in this order. See it on the tech tree →
Why it matters
The Daniell cell in The Battery gives steady current. But it must stand still, its blue copper sulfate is poisonous, and it eats its zinc slowly even when nothing is connected. For a doorbell (Electric Bells, Buzzers and Alarms), a The Telephone or a lamp you switch on now and then, you need a cell that waits for weeks doing nothing and then gives a strong burst of current. That cell is the Leclanché cell, and it needs only zinc, carbon, black manganese ore and sal ammoniac.
Put the same chemistry into a sealed zinc can as a damp paste and you get the dry cell, which works upside down, in a pocket or in the rain. With dry cells come the electric torch (flashlight), portable signal lamps, hearing aids, field telephones and radios (Radio). For a cyclist, a small dynamo turned by the tyre gives light for as long as you ride, with no cells at all.
How it works
A Leclanché cell is a zinc–carbon cell with a chemical "sponge" round the carbon:
- Negative: zinc. It dissolves into the sal ammoniac solution and leaves electrons behind, just as in The Battery.
- Positive: a rod of dense carbon, packed tightly in a mix of manganese dioxide (black manganese ore) and crushed carbon.
- Electrolyte: sal ammoniac (ammonium chloride) dissolved in water.
In a plain zinc–carbon cell, hydrogen gathers on the carbon and the voltage collapses within minutes (polarisation). Here the manganese dioxide takes up the hydrogen as it forms, so it never makes a gas film. This is called a depolariser. It works slowly, so under heavy load the voltage sags. Give the cell a rest, though, and it recovers. Sal ammoniac attacks zinc very little while no current flows, so an idle cell lasts for months.
A fresh cell gives 1.5–1.6 volts with nothing connected. That is more than a Daniell cell (1.1 V), so fewer cells are needed.
What you need
| Item | For | Notes |
|---|---|---|
| Zinc rod, sheet or can | Negative | Cast rod 10–12 mm thick, or sheet 0.4–0.6 mm (Zinc and Brass) |
| Carbon rods | Positive | Baked coke-and-tar rods, 6–10 mm thick, made as for arc lamps (The Light Bulb) |
| Manganese dioxide | Depolariser | Black manganese ore, ground to flour (below) |
| Graphite or fine coke dust | Mixed with the manganese so current can reach it | Charcoal dust is a poor substitute |
| Sal ammoniac | Electrolyte | About 150 g per wet cell |
| Zinc chloride | Dry-cell paste | Zinc dissolved in Hydrochloric Acid (Soldering and Brazing) |
| Wheat flour or starch | Thickens the paste | Grain, Flour and Bread |
| Pitch or wax | Seals | Tar, Pitch and Glue, beeswax |
| Jars, porous pots | Wet cells | Glazed and biscuit-fired pots (Pottery) |
Where to find it
Manganese ore. Look for soft, sooty-black crusts and lumps that blacken your fingers, often with fern-like black patterns on rock faces. It is common in bogs and lake beds beside iron ore, in old oxidised ore veins and in some limestones. The best mineral is pyrolusite, which is soft, black, heavy and sooty. To test it, warm a pinch with a few drops of strong Hydrochloric Acid outdoors. Good ore gives off the sharp, swimming-pool smell of chlorine (do not breathe it in). Heated red-hot in a test tube, it gives off oxygen, which makes a glowing splint burst into flame (Hydrogen, Oxygen and Gases). Ore that gives only a weak smell is poor in manganese dioxide. Pick out the lightest-coloured stone, crush the rest and grind it to flour. Wash it in water and decant the fine black mud, which removes clay.
Sal ammoniac occurs as white crusts at volcanic vents and burning coal seams. You can make it two ways:
- Bubble Ammonia gas, or the ammonia liquor from a gasworks (Coal and Coke), into Hydrochloric Acid until the smell of ammonia lingers. Then boil the liquid down to crystals.
- Mix dry ammonium sulfate (the gasworks fertiliser in Chemical Fertilisers) with an equal weight of common salt and heat the mixture in a clay pot with a cool lid. The sal ammoniac rises as white smoke and settles on the lid as a white crust (it sublimes). Scrape it off.
Method 1: The Leclanché wet cell
- Jar. A glazed jar or glass jar about 10 cm across and 15 cm tall. Rub wax or tallow round the inside of the rim. Sal ammoniac solution creeps up dry glass and crusts over everything, and grease stops it.
- Porous pot. A biscuit-fired pot, 6 cm across and 13 cm tall, as for the Daniell cell (The Battery). Stand a flat carbon plate (2 × 5 × 14 cm) or a bundle of carbon rods in the middle. It must stick out 3 cm above the top.
- Pack the pot. Mix equal volumes of ground manganese dioxide and crushed coke or carbon in pea-sized grains. Pour the mix round the carbon and tamp it hard with a stick. It must press firmly on the carbon everywhere.
- Seal the top with melted pitch, leaving one or two small holes made with a hot wire so gas can escape. Clamp a brass terminal onto the carbon. First boil the top of the carbon in wax so the salt cannot creep up it.
- Zinc. A cast zinc rod 10–12 mm thick, standing in a corner of the jar. Solder a wire to its top before it goes in.
- Fill the jar to two-thirds with sal ammoniac solution: 150 g dissolved in 1 litre of water. Do not make it stronger, because crystals will grow on the zinc.
It gives 1.5 V and up to an amp or two on a short circuit when fresh. In a bell or telephone circuit it lasts from months to a year or more. Top up the water as it evaporates. When the solution turns milky and crystals gather on the zinc, pour it out, wash the cell and refill. When the cell will no longer recover after resting overnight, repack the pot with fresh manganese.
Method 2: The dry cell
A dry cell (zinc–carbon cell) is the same cell made with no free liquid. The zinc is formed into the container, so it is both the negative plate and the can. The sal ammoniac solution is thickened into a paste. The common sizes below are worth copying, because torches and holders can then be made to fit them.
| Size | Diameter × height | Lasts (roughly) |
|---|---|---|
| Large bell cell | 64 × 152 mm | 20–30 ampere-hours |
| D (torch cell) | 34 × 61 mm | 4–8 ampere-hours at gentle current |
| C | 26 × 50 mm | About half a D |
An ampere-hour is one amp for one hour, or half an amp for two hours. A cell gives most when used gently and with rests in between. Here is how to make a D cell.
- The can. Cut zinc sheet 0.4–0.6 mm thick into a strip 110 × 58 mm. Roll it round a hardwood former 33 mm across and solder the seam outside (Soldering and Brazing; zinc chloride flux, washed off well afterward). Solder in a zinc disc as the bottom. Fill the can with water to test it; it must not seep.
- The bobbin (the positive core). Grind manganese dioxide and graphite separately to flour and sieve them through cloth. Mix 4 parts manganese dioxide to 1 part graphite by weight, or 3 to 1 if you have only coke dust. Dampen the mix with the paste liquid below until it holds together when squeezed, like damp garden soil. Stand a carbon rod 8 mm thick and 60 mm long in a split wooden mould 24 mm across. Fill round the rod and press the mix very hard with a lever or a vice (Screws, Nuts and Bolts). A loosely packed bobbin gives a weak cell. Then wrap the bobbin in one layer of thin cotton cloth and tie it with thread.
- The paste. Dissolve 30 g of sal ammoniac and 10 g of zinc chloride in 100 ml of water. For each 100 ml, stir in about 20 g of wheat flour or starch.
- Fill. Pour the cold paste into the can until it is one-third full. Push the bobbin down its middle, centred, so the paste rises to about 8 mm below its top. Stand the can in hot water (about 90 °C) for 10–15 minutes. The paste sets into a firm jelly.
- Seal. Lay a cardboard washer on the paste. Leave a gap of about 5 mm of air above it. Gas and swelling need room, or the cell bursts. Then pour melted pitch, or pitch mixed with resin, to the top, round the rod. Make one fine vent hole through the pitch with a hot needle.
- Finish. Wax the exposed top of the carbon rod. Press a brass cap onto it as the + terminal. Wrap the can in two layers of glued paper or thin card as a jacket, leaving the zinc bottom bare as the − terminal.
Let new cells rest for a day, then test them (below). Make dry cells in batches. Use them within a year or two, because they lose about a tenth of their charge each year on the shelf, faster when warm.
Batteries of cells
One cell gives 1.5 V. For more, join cells in series, the carbon of one to the zinc of the next (The Battery):
- 3 V from two D cells, inside a torch.
- 4.5 V "flat battery" from three small cells, soldered together with brass strips and set in wax in a card box. It is the classic pocket-lamp battery and makes a good bench supply.
- 9 V from six tiny cells, and 45–90 V from long rows of them, used for valve radios (The Vacuum Tube).
Join only cells of the same size and age. A weak cell in a chain drags the others down and can be driven backwards until it leaks.
The electric torch
A torch has five parts: cells, a bulb in a holder, a reflector, a switch, and a body that holds it all and carries current back from the bottom of the cells.
The body. Use a tube of brass or tinplate (Metal Pipes and Tubes, Sheet Metal and Rolling). Or roll stiff paper or card soaked in glue or varnish and run a brass strip down the inside as the return wire. For two D cells, make the bore 36 mm and the length about 175 mm. Screw a cap onto the bottom end, with a coiled steel or bronze spring (Springs) that presses the cells up and touches the bottom of the lower cell.
The bulb. You need a small bulb made for the voltage, about 2.4 V and 0.3–0.5 A for two cells, or 3.6 V for three. A carbon-filament bulb (The Light Bulb) gives perhaps one candle from two cells. It is dim, but it is a light. A tungsten filament gives about three times as much. Two D cells drive a 0.5 A bulb for roughly 3–6 hours of use, longer in short spells with rests between.
The switch. A brass slider on the outside of the body. Below it, a brass spring strip inside the body is bent so the slider pushes it against the reflector collar to make the circuit. Slide it forward to stay on. Press it without sliding to flash, for signals (Signal Fires, Flags, Semaphore and Heliographs). The contacts must wipe against each other as they close, so they scrape themselves clean.
The reflector. A bulb on its own throws light in all directions. A curved mirror called a parabola collects that light and sends it forward as a beam. Its shape follows one rule: depth = r² ÷ (4 × f), where r is the distance from the centre and f is the focal length, the point where the filament must sit. For a torch reflector with f = 10 mm:
| Distance from centre | 5 mm | 10 mm | 15 mm | 20 mm | 25 mm |
|---|---|---|---|---|---|
| Depth of the curve | 0.6 mm | 2.5 mm | 5.6 mm | 10 mm | 15.6 mm |
Mark these depths on a card and cut a template. Turn a hardwood former to fit it on the The Lathe. Then spin a disc of soft brass or copper sheet over the former: press it against the turning wood with a rounded hardwood stick, a little at a time, oiling as you go. Cut a hole at the centre for the bulb. Polish the inside and silver it (Mirrors) or nickel-plate it (Electroplating). A pressed or spun reflector 50–60 mm across suits a D torch. Cover the front with a flat glass disc 2 mm thick, held by a screwed ring.
Focusing. Shine the torch on a wall 3 m away. Slide the bulb in or out 1–3 mm until the spot is smallest and brightest, then fix it. If the beam has a dark hole in the middle, the filament is too far forward. A wide, dim ring means it sits too far back.
The bulb holder
A bulb holder holds a lamp firmly, connects both its contacts, and keeps them apart.
- Spring clip holder, the simplest. Two brass strips on a block of insulator. One presses on the bulb's centre contact, and a curved one grips its side contact.
- Screw holder. A brass tube with a screw thread inside, and a sprung brass tongue at the bottom that touches the centre contact. To make the thread without a tap, wind brass wire round a bulb base to the right pitch, slip the coil inside a brass tube and solder it there. The tube and thread form one contact and the tongue the other. A disc of insulator separates them.
- Bayonet holder. For room lamps (Wiring and Electrical Safety). A brass sleeve with two L-shaped slots takes two pins on the lamp cap. Two spring-loaded plungers press on the lamp's two contacts.
Insulators: fired clay or porcelain (Stoneware and Porcelain), mica, hardwood boiled in wax, or later moulded plastic (Early Plastics). Good or bad? Tap the lit lamp with a pencil. It must not flicker. The bulb must not wobble, and no brass of one contact may come within 2 mm of the other.
The bicycle dynamo
A The Bicycle can make its own light. A small The Generator presses on the tyre, and the faster you ride, the faster it spins.
The bottle dynamo is a sealed case about 35–40 mm across and 75–90 mm long, on a spring-loaded hinge fixed to the fork.
- Rotor. A permanent magnet of hardened steel (Magnets), shaped as a short bar or a star of 4–8 poles, on a steel spindle. It turns in two small Making Ball and Roller Bearings or oiled bronze bushes (Bearings and Lubrication).
- Stator. Soft-iron pole pieces close round the magnet, with 0.5–1 mm of clearance, and lead its magnetism through a coil. Wind about 500–1,000 turns of 0.3 mm insulated wire (Copper Wire). One end goes to the terminal, the other to the case, and the case is earthed to the frame.
- Roller. A knurled steel or ribbed rubber roller about 20 mm across on the spindle. At 15 km/h it spins about 4,000 times a minute.
- Mounting. Point the dynamo's axis straight at the wheel hub, so the roller runs square on the tyre wall. A slanting roller slips in the wet and wears the tyre. A latch holds it off the tyre in daylight.
The standard output is 6 V and 3 W: a 2.4 W front lamp and a 0.6 W red tail lamp. The output is alternating current, which bulbs do not mind. A useful quirk: as speed rises, the coil's own magnetic resistance to changing current rises too. So above about 10 km/h the current stays nearly constant at about half an amp whatever the speed. That is what keeps the bulbs from burning out downhill. It is also why, when the tail bulb fails, the front bulb soon follows: it now takes all the current. Replace both together.
Steel magnets are weak and lose strength if the rotor is pulled out of its iron. Keep the dynamo assembled, and make the magnet as large as fits. The hub dynamo, built into the front-wheel hub, does the same job with no slipping and less drag.
Good or bad? Spin the wheel by hand. The lamp should glow at walking pace and be at full brightness by a steady riding speed. You should hardly feel the drag on a level road.
How to tell it worked
- Open voltage. Compare a new cell with a known good one on a galvanometer (Measuring Electricity). A fresh Leclanché or dry cell reads about one and a half times as high as a Daniell cell.
- Under load. Light a torch bulb from the cell. It should be bright at once and stay bright for a minute. A cell whose bulb fades within seconds has a loose or too-thin bobbin. A dead cell gives under about 1 V under load.
- Recovery. A Leclanché cell that has sagged under load climbs back to full voltage after half an hour of rest.
Note Troubleshooting. Low voltage from the start → poor manganese ore. Test it for chlorine as above, or use more graphite. Strong at first, then quickly weak → bobbin packed loosely, or too little graphite. White crust all over the wet cell → solution too strong, or the jar rim and the carbon not waxed. Dry cell leaks or swells → no air gap under the seal, or it was run flat and left. Remove dead cells from torches. Zinc can eaten through in months → impure zinc, or iron dust in the mix. Use clean zinc and grind with stone, not iron. Torch flickers → dirty switch or holder contacts, or a weak spring. Clean them and stretch the spring. Bicycle lamp dim when wet → roller slipping; increase the spring pressure and check alignment.
Dangers
Warning Chlorine. Testing manganese ore with acid gives off chlorine, which damages the lungs. Use a pinch, outdoors, and do not lean over it. See Chlorine and Bleach.
Warning Acid, hydrogen and fumes. Making zinc chloride means dissolving zinc in Hydrochloric Acid, which burns skin and eyes and gives off hydrogen that explodes from a spark or flame. Zinc chloride itself burns skin and eyes. Subliming sal ammoniac gives off choking white fumes. Do all three outdoors, with eye protection, no flames nearby, and water at hand to wash splashes.
- Sal ammoniac and cell paste irritate the eyes and stomach. Keep cells away from small children, who may chew them. Wash your hands after making cells.
- Never try to recharge dry cells with a strong current. They heat, swell and can burst and spray hot paste.
- Short circuits. A big bell cell or a battery of cells shorted by a wire or a key in a pocket can make the wire red-hot. Tape or cap the terminals of spare cells.
- Mercury. Old makers coated the zinc with mercury to slow corrosion. Do not do this; it poisons the people who make the cells and the ground where they are thrown away (Mercury).
What this unlocks
Leclanché cells run doorbells, alarms and telephone sets (Electric Bells, Buzzers and Alarms, The Telephone). Dry cells make electricity portable: torches, signal lamps, field telephones, the first portable Radio sets and their high-voltage batteries (The Vacuum Tube), and later hearing aids and test meters (Measuring Electricity). For heavy current that can be recharged, use the The Rechargeable Battery. Much later, a light-emitting diode in place of the filament bulb lets a torch run many times longer on the same cells. The parabolic reflector also gives car headlamps and the searchlight (Arc Lamps, Neon and Fluorescent Lights).
How it was first done
Georges Leclanché, a French engineer, made his cell in 1866. Within two years it was being used by the Belgian telegraph service, and it ran most of the world's doorbells and telephone sets for half a century. In 1886–87 Carl Gassner in Germany patented a dry version with a zinc can and a paste of plaster and zinc oxide. Wilhelm Hellesen in Denmark made a similar cell at about the same time. The Columbia cell (1896), 6 inches tall, was the first dry cell sold to the public in large numbers. In 1899 David Misell made the first tubular electric torch for Conrad Hubert's company in New York, which later became Eveready. Its carbon-filament bulbs were so weak that it could only be switched on briefly, which is why it was nicknamed the "flash light". Bicycle dynamos appeared around the turn of the twentieth century and were common across Europe by the 1930s.
Source: content/entries/electricity/dry-cells-and-torches.md